Perfluoro amphoteric ion exchange resin, ion membrane and preparation method thereof
By introducing perfluorinated anion and cation structural units into the perfluoroamphoteric ion exchange resin to form an acid-base ion pair, the problem of low proton conductivity and swelling of the perfluorosulfonic acid proton exchange membrane at high temperatures is solved, and the mechanics and performance of the membrane are improved. Conductivity properties.
Patent Information
- Application Number
- CN202211726756.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The existing perfluorosulfonic acid proton exchange membrane has low proton conductivity under high temperature and low humidity conditions, and is prone to swelling problems, resulting in reduced mechanical strength and ion selectivity, making it difficult to meet the needs of high temperature applications.
It uses perfluorinated amphoteric ion exchange resin, which contains both perfluorinated anion and cation structural units in its structure. It forms an acid-base ion pair through the acid-base exchange process, enhances the interaction force, inhibits the water absorption of the sulfonic acid group, and combines the Donnan exclusion effect. , improve the mechanical properties and proton conductivity of the membrane.
It achieves maintaining high ionic conductivity and mechanical properties under high temperature conditions, solves the problem of excessive swelling and selectivity of the membrane, and ensures structural stability and conductivity performance in high temperature and low humidity environments.
Smart Images

Figure CN116284537B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials and relates to a perfluoro zwitterionic resin, an ion membrane and a preparation method thereof. Background Art
[0002] Perfluorosulfonic acid proton exchange membrane (PFSA) is an ion exchange resin with a single cation exchange function. Its main chain structure is a strongly hydrophobic polytetrafluoroethylene (Teflon) skeleton, and the side chain has a single hydrophilic cation exchange group (-SO3 - , negatively charged groups) on the side chains of the perfluorosulfonic acid resin. The hydrophilic cationic groups on the side chains of the perfluorosulfonic acid resin and the hydrophobic main chain structure will undergo a hydrophilic / hydrophobic microphase separation, thereby forming nanoscale sulfonic acid ion clusters that are evenly distributed in the continuous CF lattice (polymer crystal region). Under working conditions, the transfer of ions in PFSA is conducted through the sulfonic acid groups reacting with water to form hydrated protons.
[0003] However, the strong water absorption of the sulfonic acid groups in the membrane will cause an expansion-de-expansion process, resulting in serious swelling problems, which will cause the membrane to deform and even cause problems such as pinholes or cracks, significantly reducing the mechanical strength of the membrane. In addition, severe swelling problems will reduce the ion selectivity of the ion exchange membrane, such as the permeation of hydrogen in fuel cells, the permeation of methanol, and the permeation of vanadium ions in vanadium batteries, which will reduce the selectivity of cations and reduce the energy efficiency of the battery. Due to the microphase separation structure of the PFSA membrane, ions need to rely on the ion transmission channel formed by the hydrophilic phase during the transmission process, but the currently used PFSA membrane can only have good proton conductivity at lower temperatures (not higher than 80°C) and higher humidity. Therefore, when the operating temperature is higher than 100°C, its ion proton conductivity will be far lower than 0.01S / cm, which can no longer meet the requirements of ion conduction.
[0004] In view of the above problems existing in the current PFSA membrane, current research mainly focuses on inorganic particle doping, organic-inorganic composite, and chemical crosslinking methods to improve the membrane's ion selectivity, high swelling degree, high temperature resistance, etc. For example, patent CN101667648A discloses a method for preparing a water-retaining proton exchange membrane for a fuel cell, which effectively fills the pores of an expanded polytetrafluoroethylene microporous film with a perfluorosulfonic acid resin component and a water-retaining silica component by a combined dipping-spraying method. However, this method has the problems that silica is easy to agglomerate, the stability of the obtained proton exchange membrane is poor, and the preparation method is relatively complicated and the proton conductivity of the obtained proton exchange membrane is still not ideal. Patent CN111100328A discloses a modified inorganic nanoparticle, polymer mixed slurry, composite membrane and preparation method, which improves the water retention performance of the composite membrane and avoids the agglomeration of inorganic nanoparticles by modifying inorganic nanoparticles with phosphoric acid groups. However, the phosphoric acid groups used in this method have a corrosive effect on the membrane. When hydrogen protons are transferred to hydrates, the phosphoric acid groups are also easily transferred with the hydrates, thereby reducing the proton conductivity to a certain extent. Patent CN111370723A improves the ion selectivity of the membrane in vanadium flow batteries by adding lanthanum oxide, cerium oxide, yttrium oxide or cobalt oxide. However, the additives in the membrane are in a free mode. These membranes are often leached by additives during operation, resulting in a decrease in proton conductivity.
[0005] The high-boiling acid doped in the doped zwitterionic ion exchange membrane is easy to lose, and the blended zwitterionic ion exchange membrane has the problem of component compatibility. Compared with them, the intrinsic zwitterionic ion exchange membrane shows good development prospects. However, the main chain of the current PFSA membrane is an ultra-stable Teflon skeleton, which is difficult to graft ionic groups; in addition, the number of reactive groups that can react on the side chain is small. The above reasons make it more difficult to synthesize intrinsic zwitterionic ion exchange resins and ion membranes. At present, conventional intrinsic zwitterionic ion exchange membranes are mostly prepared by irradiation modification methods. Severe modification conditions can cause the base membrane to be unstable or chemically degraded. Therefore, it is particularly important to develop zwitterionic ion exchange membranes with good synthesis performance. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a perfluoro amphoteric ion exchange resin, an ion membrane and a preparation method thereof.
[0007] In order to achieve the above purpose, the following technical solutions are adopted:
[0008] A type of perfluoro amphoteric ion exchange resin, characterized in that the resin structure contains both perfluoro anion structural units (negatively charged groups) and perfluoro cation structural units (positively charged groups), and the resin has a structure shown in the following formula I:
[0009]
[0010] In the structural formula (I), ad is an integer of 0 to 30, x is 0 or 1; y, z are integers of 0 to 3, preferably a, c are 1 to 10; b, d = 1; x = 1; y, z = 0, 1; e is the number of repeating units, and e is 50 to 10000; a+b / (a+b+c+d) = 0.05 to 0.9; c+d / (a+b+c+d) = 0.1 to 0.95; preferably a+b / (a+b+c+d) = 0.15 to 0.65; c+d / (a+b+c+d) = 0.35 to 0.85; further preferably a+b / (a+b+c+d) = 0.5 to 0.8; c+d / (a+b+c+d) = 0.2 to 0.5;
[0011] Among them, in the perfluorinated anion structural unit, the negatively charged group is -SO3-, and the counter ion M is H + , Li + , Na + , K + , Ag + , NH4 + , NH3 + ,Mg 2+ 、Al 3+ , Ca 2+ , Ba 2+ , Fe 2+ , Fe 3+ , Cu 2+ 、Zn 2+ , Mn 2+ One of the above, preferably M is H + , K + , Li + , NH4 + .
[0012] Among them, in the perfluorinated cationic structural unit, at least one of the positively charged groups is a cationic group Ar1, and the cationic group structure contains one or more or A group, the structure of which is shown in Formula II;
[0013]
[0014] Preferably, the cationic group structure is selected from one of Formula III:
[0015]
[0016] Among them, the counter ion Ar2 in the perfluorinated cation structural unit is Cl - ,Br - , I - , F- , NO3 - , OH - , HCO3 - ,CO3 2- , CH3COO - , SCN - , SO4 2- , HSO3 - , HSO4 - , ClO4 - , S2O3 2- , C2O4 2- , HSO4 - , PF6 - , BF4 - ,[C(CN)3] - , [(FSO2)2N] - , [(CF3SO2)2N] - , [B(CN)4] - , [(C2F5)3PF3] - , (H2PO4) - , (H2PO3) - , [(H2PO4) - (H3PO4) n , n>1],(H2PO4) - , HSO3 - , SO3 - , preferably Ar2 is Cl - , OH - , [(CF3SO2)2N] - , (H2PO3) - , [(H2PO4) - (H3PO4) n , n>1].
[0017] The resin structure also contains tetrafluoroethylene polymerization units, and the molar content percentages of the various polymerization units in the copolymer are: the overall molar fraction of tetrafluoroethylene polymerization units is 5-85%, the overall molar fraction of perfluoro anion units is 10-90%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 5-65%. Preferably, the molar content percentages of the various polymerization units in the copolymer are: the overall molar fraction of tetrafluoroethylene polymerization units is 45-51%, the overall molar fraction of perfluoro anion units is 35-40%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 10-19%.
[0018] The ion exchange capacity of the resin is 0.5 to 2.5 mmol / g, preferably 0.9 to 1.6 mmol / g, and more preferably 0.9 to 1.4 mmol / g.
[0019] The present invention also provides a method for preparing the above-mentioned perfluoro amphoteric ion exchange resin, wherein the preparation method is selected from one of the following methods:
[0020] (Method 1)
[0021] (1-1) A perfluorovinyl ether sulfonyl fluoride resin (PFSO2F) is subjected to a one-step grafting reaction with an Ar reagent having a tertiary amine or tertiary phosphorus group in an organic solvent to graft a cationic group to synthesize an intermediate product; or, PFSO2F is first pre-swollen in an organic solvent, and then subjected to a grafting reaction with an Ar reagent to graft a cationic group to synthesize an intermediate product;
[0022] (1-2) The obtained intermediate product is subjected to ion exchange by post-treatment with an alkali, acid, or salt containing M ions, and the unreacted sulfonyl fluoride group -SO2F is converted into a perfluorosulfonic acid group -SO3M. After washing and drying, a perfluoro amphoteric ion exchange resin is obtained. The reaction formula is as follows:
[0023]
[0024] The obtained ion resin can be post-treated with acid, alkali or salt to complete the ion exchange according to the type of counter ion of the cation group it carries.
[0025] The Ar reagent is a reagent containing one or more tertiary amines or tertiary phosphorus structures, and its general structural formula is shown in Formula IV:
[0026]
[0027]
[0028] Further preferably, the structure of the Ar reagent is one of the structures shown in Formula V:
[0029]
[0030] (Method 2)
[0031] PFSO2F is pre-swollen in an organic solvent and reacted with ammonia, with a molar ratio of resin to ammonia of 1:15; part of the -SO2F groups are converted into -SO2NH2, and after the reaction, the remaining -SO2F groups are converted into -SO3H through an acid-base treatment process to obtain a structural unit containing both -SO3H and -SO2NH2, thereby forming -SO3 - HN +HSO2-acid-base ion pair, after washing and drying, amphoteric ion exchange resin is obtained; or PFSO2F is pre-swollen in an organic solvent and reacted with ammonia, with a molar ratio of resin to ammonia of 1:15; part of the -SO2F group is converted into -SO2NH2 to obtain an intermediate product, and then the intermediate product is grafted with a Q-Ar reagent with a cationic group in an organic solvent for grafting the cationic group, and finally the remaining -SO2F group is converted into -SO3M through an acid, base, and salt ion exchange process, and amphoteric ion exchange resin is obtained after washing and drying; the reaction formula is as follows:
[0032]
[0033] Preferably, when the counter ion in the cationic group is Cl - Br - ,I - When acid, base, and salt ion exchange is carried out, the exchange is OH - , [(CF3SO2)2N] - , (H2PO3) - wait.
[0034] The Q-Ar reagent is a reagent with one or more quaternary amine or quaternary phosphonium structures, and its general structural formula is shown in Formula VI, wherein at least one of R1 to R4 is a cationic group containing one or more, and the structure of the cationic group is shown in Formula II. The remaining substituent groups in the structure are one of -F, -Cl, -H, -Br, -OH, -CH3, -OCH3, -Ph (Ph represents a benzene ring), -OPh, -CH2Cl, -CH2Br, and -CH2CH3;
[0035]
[0036] Further preferably, the structure of the Q-Ar reagent is one of the structures shown in Formula VII:
[0037]
[0038] Preferably according to the present invention, the organic solvent in the preparation method is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, ethanol, isopropanol, dimethyl sulfoxide or ethyl acetate.
[0039] Preferably, according to the present invention, the molar ratio of the perfluorosulfonyl fluoride resin to the monomer reagent of the Ar reagent in method (1) is 1:5-20; the molar ratio of the resin precursor to the monomer reagent of the Q-Ar reagent in method (2) is 1:3-20, preferably 1:8-10.
[0040] Preferably according to the present invention, the mass volume ratio of PFSO2F resin to organic solvent in methods (1) and (2) is 1:1 to 12 g / mL; more preferably 1:1 to 6 g / mL; most preferably 1:1 to 3 g / mL.
[0041] According to the preferred embodiment of the present invention, the temperature of the grafting reaction in the method is 15 to 150° C., preferably 25 to 80° C.; more preferably 30 to 80° C.; the reaction time is 1 to 48 hours, preferably 5 to 12 hours.
[0042] Preferably, according to the present invention, the pre-swelling in method (1) is to swell the perfluorosulfonyl fluoride resin in an organic solvent at 40 to 50° C. for 60 to 300 minutes.
[0043] According to the preferred embodiment of the present invention, in the acid, base and salt ion exchange process, the base is one of sodium hydroxide, triethylamine, trimethylamine, ammonia water and potassium hydroxide, and the concentration is 5-50wt%, preferably 15-40wt% of sodium hydroxide; the acid is one of hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid and nitric acid, and the concentration is 5-50wt%, preferably 25-40wt% of sulfuric acid or nitric acid; the salt is one of potassium chloride, lithium hexafluorophosphate, lithium hypochlorite, lithium tetrafluoroborate, lithium bistrifluoromethanesulfonyl imide, ammonium chloride, sodium sulfate, ammonium sulfate, ammonium carbonate, ammonium nitrate, sodium phosphate and sodium nitrate, and the concentration is 5-50wt%, preferably 15-50wt% of sulfuric acid or nitric acid.
[0044] According to the preferred embodiment of the present invention, the temperature of the acid, base and salt ion exchange process in the method is 30-100° C., preferably 50-80° C.; the reaction time is 1-48 hours, preferably 8-12 hours.
[0045] Preferably according to the present invention, the washing in the preparation method adopts deionized water washing, and the drying is carried out at 55-65° C. for 18-36 hours.
[0046] The perfluoro amphoteric ion exchange resin prepared above can determine the ion exchange capacity and the proportion of perfluoro anion and perfluoro cation structural units by acid-base titration. According to the requirements of product performance, the grafting rate of the reaction can be controlled by adjusting the reaction time, reaction temperature and raw material ratio in the preparation method, thereby adjusting the ion exchange capacity of the resin and the proportion of each unit.
[0047] Another object of the present invention is to provide a method for preparing a perfluoro zwitterionic ion exchange membrane, characterized in that the ion membrane structure contains a perfluoro zwitterionic ion exchange resin component. In particular, the molar content percentage of the perfluoro zwitterionic ion exchange resin in the membrane is 1 to 100%. The perfluoro zwitterionic ion exchange membrane of the above structure has a thickness of 5 to 250 μm, preferably 8 to 150 μm, more preferably 8 to 50 μm, and a thermal degradation temperature of 255 to 350°C.
[0048] The method for preparing the perfluorinated zwitterionic ion exchange membrane is characterized in that the molar content of the perfluorinated anion structural unit in the ion membrane is 5 to 95%, and the molar content of the perfluorinated cation structural unit is 5 to 80%. The method for preparing the ion membrane is selected from one of the following methods:
[0049] Preparation method of homogeneous perfluorinated zwitterionic membrane:
[0050] a) Preparation of perfluoro anion exchange resin: Referring to methods (1) (2), perfluorovinyl ether sulfonyl fluoride resin (PFSO2F) is subjected to acid, alkali and salt ion exchange processes to convert all -SO2F into perfluorosulfonic acid groups -SO3M to obtain a perfluoro anion exchange resin (structure as shown in Formula I, except that d=0 in the structure).
[0051] b) Preparation of mixed perfluoro zwitterionic resin: fluorinated anion exchange resin and perfluoro zwitterionic resin are mixed to obtain the mixed perfluoro zwitterionic resin, wherein the molar content percentage of each polymer unit in the mixed perfluoro zwitterionic resin is as follows: the molar content percentage of perfluoro anion exchange resin is 0-99%, and the molar content percentage of perfluoro zwitterionic resin in the membrane is 1-100%.
[0052] c) dissolving the mixed perfluorozwitterionic resin obtained in step (b) with a solvent to obtain a uniform film-forming solution;
[0053] d) forming a film on glass or a porous fiber reinforced layer material by solution casting, solution pouring, wire rod coating, doctor blade coating, spraying or dipping the membrane-forming liquid, pre-drying at 80-90° C., drying at 140-150° C. for 90-100 min, taking out and demolding, and obtaining a homogeneous perfluorozwitterionic membrane.
[0054] The solid content of the membrane-making solution in step 1) is 5 to 35 wt.%, and the solvent can be one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, butanone, alcohols with 1 to 5 carbon chains, aqueous solutions of alcohols with 1 to 5 carbon chains, formic acid or acetic acid.
[0055] The overall thickness of the porous fiber reinforced material is 2 to 50 μm, preferably 10 to 20 μm. The number of layers of the porous fiber reinforced material is 1 to 35 layers, preferably 1 to 15 layers, and more preferably 1 to 8 layers. The porosity of the porous fiber reinforced layer material is 60% to %, preferably 75% to 95%, and more preferably 80% to 95%. The gram weight of the porous fiber reinforced material is 2 to 6 g / m 2 , preferably 2.5 to 5 g / m 2 .
[0056] Preferably, the porous fiber reinforcement material is selected from one or more of olefin polymers containing halogen atoms, olefin polymers, fluorinated olefin-olefin copolymers, perfluoroalkyl vinyl ether copolymers, acetate fibers, amide polymers, inorganic fibers, etc. More preferably, it is one or more of polytetrafluoroethylene, polyvinylidene fluoride, and poly(vinylidene fluoride-co-hexafluoropropylene).
[0057] Heterogeneous perfluorinated zwitterionic membrane:
[0058] e) preparing a polymer base film by melt extruding a perfluorovinyl ether sulfonyl fluoride resin (PFSO2F) at an extrusion temperature of 200 to 310° C.;
[0059] f) According to method (1) (2), a solid-liquid reaction is carried out based on the PFSO2F solid-state base film to construct a perfluorozwitterionic polymer structure;
[0060] g) converting the remaining -SO2F groups in the base membrane into -SO3M through an acid, base and salt ion exchange process, and obtaining a heterogeneous perfluorozwitterionic membrane after washing and drying.
[0061] Compared with the prior art, the present invention has at least the following advantages:
[0062] 1. The cationic structural unit introduced into the zwitterionic ion exchange resin and membrane structure provided by the present invention has a low water absorption rate, and can form an ion pair with the anionic structural unit (an acid-base ion pair is formed between positive and negative charges), thereby enhancing the interaction between the two units, effectively limiting the strong water absorption of the sulfonic acid group in the ion membrane, and greatly enhancing the mechanical properties of the membrane, solving the problem of excessive swelling of the membrane. By adjusting the reaction time, the ratio of the perfluorinated anionic structural unit to the perfluorinated cationic structural unit is controlled.
[0063] 2. Benefiting from the Donnan exclusion effect (positive charges repel each other), the introduction of cationic structural units into the resin and membrane structure can effectively inhibit the penetration of positively charged ions in the zwitterionic membrane, and has excellent alcohol and vanadium resistance properties. In addition, the breaking and formation of hydrogen bonds between acid and base structures can also transfer protons (Grotthuss mechanism), which helps to improve the proton conduction rate of the ion membrane, thereby achieving the purpose of balancing the conductivity and ion permeability of the membrane.
[0064] 3. The cationic unit in the zwitterionic membrane provided by the present invention can spontaneously assemble with the acidic unit (sulfonic acid, phosphoric acid) to form an acid-base ion pair. Especially in the absence of water or anhydrous conditions, protons can be transferred between the donor and the acceptor based on the Grotuss mechanism without the need for water molecules.
[0065] 4. The zwitterionic membrane provided by the present invention has an ionic conductivity higher than 0.02S / cm when measured at high temperature (120-150°C), and has a more stable structure. The sulfonic acid structural unit ensures the performance at low temperature (100°C).
[0066] 5. The ion exchange membrane contains both perfluorinated anion structural units (negatively charged groups) and perfluorinated cation structural units (positively charged groups), and has excellent ion selectivity and high conductivity; it can maintain high dimensional stability under low temperature and high humidity (0℃-100℃, 100% relative humidity); it can still have higher structural stability, good mechanical properties and chemical properties under high temperature (120℃-150℃) and low humidity environment. It can be applied to redox flow batteries, water electrolysis hydrogen production and low temperature / high temperature hydrogen fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 : is the infrared test spectrum of each resin in the embodiment, wherein A is PFSO2F resin, B is resin A3, C is resin A1, and D is resin A4;
[0068] Figure 2 It is a device for testing the vanadium ion permeability of membranes. DETAILED DESCRIPTION
[0069] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.
[0070] The present invention is described in detail below in conjunction with specific examples, which are only used to illustrate the present invention in detail and are not used to limit the scope of protection of the present invention. The present invention is not limited to the following embodiments, and other combination schemes derived on the basis of the present invention all belong to the scope of protection of the present invention. The raw materials and reagents involved in the examples, unless otherwise specified, are all common commercially available products; the experimental methods involved in the examples, unless otherwise specified, are all conventional technical means in the art.
[0071] The wavy line of the present invention represents an alkyl chain or perfluoroalkyl chain of any length or H. The length is schematic and does not represent the actual length.
[0072] In the examples, the resin adopts Fenton test to accelerate the oxidation of target products, so as to achieve the purpose of examining the chemical stability of the resin. The chemical stability of the polymer is evaluated by testing the retention rate (RV%) of IEC of the polymer before and after the Fenton test.
[0073] The specific conditions of the Fenton experiment are: 20ppm Fe 2+ Ions are added to 30wt% H2O2 to prepare Fenton's reagent. Then the polymer is immersed in Fenton's reagent in a water bath at 80℃. After a certain period of immersion, the IEC of the polymer is tested to determine the chemical stability of the polymer. In order to ensure the concentration of ·OH free radicals, the Fenton's reagent needs to be replaced every 3 hours.
[0074] Titration of ion exchange capacity (IEC): Accurately weigh a certain weight of the dry target product, and then use a 1M NaCl aqueous solution for ion exchange for more than 12 hours. Collect the ion exchange solution, use phenolphthalein as an indicator, and titrate with 0.1M NaOH standard solution until the solution turns pink. The ion exchange capacity (IEC) value of the target product can be calculated according to the following formula:
[0075] IEC=(V NaOH ×C NaOH ) / m
[0076] Where: V NaOH ——The volume of NaOH standard solution consumed, mL; C NaOH ——molar concentration of NaOH standard solution, mmol / mL; m——mass of dry target product, g.
[0077] IEC retention rate:
[0078] RV%=(IEC1-IEC0) / IEC0
[0079] Where:
[0080] IEC1 and IEC0 represent the IEC of the polymer before and after the Fenton test, respectively.
[0081] The mechanical properties test of the ion membrane is carried out in accordance with GB / T20042.3-2009.
[0082] The ion membrane conductivity test was carried out in accordance with GB / T20042.3-2009 (the test conditions were room temperature and 120°C).
[0083] Thermal degradation temperature (defined as the temperature at which the polymer degrades 5%): The test was conducted using a thermogravimetric analyzer, TAQ50 produced by Perkin Elmer, USA, with a N2 atmosphere, a heating rate of 10°C / min, and a temperature range of 50-800°C. The samples were dried at 60°C for 24 hours before testing.
[0084] Water absorption and swelling degree: Soak the sample in deionized water at the test temperature (test conditions are room temperature and 80°C) for 24 hours to ensure complete swelling. Take out the sample, quickly wipe off the water on the surface of the sample, and record the sample weight (M w ) and length (L w Then the sample was dried at 80°C and the sample weight (M d ) and length (L d ), water absorption and swelling degree are calculated by the following formula:
[0085] Water absorption % = [(M w -M d ) / M d ]×100%, swelling degree %=[(L w -L d ) / L d ]×100%.
[0086] Vanadium ion permeability of ion membrane: Figure 2 The device shown (refer to Chinese patent CN 114835842 A) tests the vanadium ion permeability of the membrane. The two sides of the container are 3MH2SO4 / 1.5MVOSO4 and 3MH2SO4 / 1.5MMgSO4 respectively, and the ion membrane to be tested is in the middle. Mechanical stirring is auxiliary on both sides of the container to prevent concentration polarization. As time goes by, samples are taken from the electrode solution on the right at regular intervals to test the VOSO4 concentration, and an equal amount of stock solution is added. The VOSO4 concentration test is tested by an ultraviolet spectrophotometer (JASCO, FT-IR4100, Japan), and the vanadium ion permeability is calculated by referring to the literature (Journal of Membrane Science 525 (2017) 229–239).
[0087] Embodiment 1:
[0088] A preparation method of a perfluoro amphoteric ion exchange resin, wherein triethylamine (TEA) is selected as an Ar reagent, and a cationic group is grafted onto the resin by a grafting reaction according to method (1). PFSO2F resin (a'=6, b'=1; x, y, z=1, number average molecular weight of 400,000, molar equivalent E w =1000g / mol), the specific steps are as follows:
[0089] (1) After cleaning a 500mL sealed reactor, evacuate the reactor and replace it with high-purity nitrogen three times, add 50g PFSO2F resin and 100mL dry N,N-dimethylacetamide, turn on the stirring device, slowly heat to 50℃ and maintain for 60min to swell the resin. Then add 0.06g triethylamine, and the molar ratio of PFSO2F to TEA is about 1:5; after the addition is completed, react at 60℃ with mechanical stirring for 5h and then cool to room temperature. The pressure in the reactor is controlled below 0.2MPa. After the reaction is completed, the -SO2F group is partially converted into -SO2Et3N, the product is filtered, and the excess triethylamine is washed with deionized water; finally, it is dried at 60℃ to obtain the intermediate product.
[0090] (2) The intermediate product is immersed in a 15% KOH solution at 60°C for 24 hours to completely convert the counter ions in the cationic group into hydroxide ions, and the remaining -SO2F is converted into -SO3K. The product is washed with deionized water to remove excess triethylamine; finally, it is dried at 60°C to obtain a perfluoro amphoteric ion exchange resin, denoted as A1, and the reaction formula is as follows:
[0091]
[0092] The infrared transmission spectrum of product A1 was measured. Figure 1 PFSO2F( Figure 1 , A) and A1( Figure 1 , C) is the infrared characterization result diagram. It can be seen from the figure that at 1467cm -1 There is an obvious infrared absorption peak attributable to the sulfonyl fluoride group (-SO2F) at the position of the product. The infrared absorption peak of the -SO2F group disappears in the obtained product. -1 The characteristic peaks of -CH2 and -CH3 appeared at 1478cm -1 Department The characteristic peak at 1060cm -1 -SO3 appeared nearby - The above results prove that the amphoteric ion exchange resin A1 was successfully synthesized.
[0093] After ion exchange capacity (IEC) measurement, the ion exchange capacity (IEC) of the obtained target product A1 is 1.00 mmol / g, and in the structure of the obtained target product A1, a+b / (a+b+c+d)=0.80; c+d / (a+b+c+d)=0.20.
[0094] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 50.50%, the overall molar fraction of perfluoro anion units is 39.30%, and the overall molar fraction of perfluoro cationic structural units is 10.2%.
[0095] Embodiment 2:
[0096] Preparation of a perfluoro amphoteric ion exchange resin, the target product A1 prepared in Example 1 was immersed in 25wt% sulfuric acid at 60°C for 20h to complete ion exchange, -SO3K was completely converted into perfluorosulfonic acid groups -SO3H, and the counter ion in the cationic group was converted into -HSO4 - The product was washed with deionized water and dried at 60°C for 30h to obtain the target product, denoted as A2, in which a+b / (a+b+c+d)=0.80; c+d / (a+b+c+d)=0.20, IEC is 0.90mmol / g, and its structure is as follows:
[0097]
[0098] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 50.10%, the overall molar fraction of perfluoro anion units is 38.30%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 11.60%.
[0099] Embodiment 3:
[0100] A preparation method of a perfluoro amphoteric ion exchange resin is to graft a cationic group by grafting reaction according to method (2). PFSO2F resin (a'=4, b'=1; x, y, z=1, number average molecular weight of 410,000, molar equivalent E w =869g / mol), the specific steps are as follows:
[0101] (1) A 500 mL sealed reactor was cleaned, evacuated and replaced with high-purity nitrogen three times, and then 50 g of PFSO2F resin and 150 mL of dry N,N-dimethylacetamide were added. The stirring device was turned on and slowly heated to 50°C and maintained for 60 min. The product was filtered and repeatedly washed with deionized water three times to obtain a pre-swollen resin.
[0102] (2) The reactor was cleaned and evacuated again, and then replaced with high-purity nitrogen three times. Then, the pre-swollen resin and 200 ml of 10% ammonia solution were added. The stirring device was turned on and slowly heated to 30°C and maintained for 120 min. The pressure in the reactor was controlled below 0.15 MPa. Part of the -SO2F group was converted into -SO2NH2 (the reaction degree was controlled by the reaction time, and then the -SO2F reaction degree was determined by titration of IEC). The product was filtered and repeatedly washed with deionized water three times. It was immersed in 15% KOH and 25wt% sulfuric acid solutions at 70°C for 24 h to complete ion exchange. The remaining -SO2F was converted into -SO3H. The obtained resin structure contained both -SO3H and -SO2NH2 structural units, thereby forming -SO3 - HN + HSO2-acid-base ion pair, thus forming -SO3 - HN + HSO3 - Acid-base ion pair, the product is washed with deionized water; finally dried at 60°C to obtain a perfluoro amphoteric ion exchange resin, denoted as A3, and the reaction formula is as follows:
[0103]
[0104] The product A3( Figure 1 , B) Infrared transmission spectrum measurement, it can be seen that in the range of 3304-3400cm -1 and 1548cm -1 The characteristic peaks of -SO2NH2 primary amine (-NH2 group) are between 1060cm -1 -SO3 appeared nearby - The characteristic peak (-SO3H group) of
[0105] After ion exchange capacity (IEC) measurement, the IEC of the obtained target product A3 is 1.15 mmol / g, and in the structure of the obtained target product A3, a+b / (a+b+c+d)=0.73; c+d / (a+b+c+d)=0.27.
[0106] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 49.00%, the overall molar fraction of perfluoro anion units is 37.50%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 13.50%.
[0107] Embodiment 4:
[0108] A perfluoro amphoteric ion exchange resin is prepared by grafting cationic groups through a grafting reaction according to method (2). 10g of the product A3 obtained in Example 3 was added to 200mL of dry N,N-dimethylacetamide, the stirring device was turned on, and it was slowly heated to 80°C. After it was completely dissolved, 0.04g of 1-allyl-3-methylimidazolium chloride was added, and the molar ratio of the intermediate product to 1-allyl-3-methylimidazolium chloride (Q-Ar reagent) was about 1:10; after the addition was completed, the amino group in -SO2NH2 was used for Aza-Michael reaction to graft the cationic group under mechanical stirring at 80°C, and the product was cooled to room temperature after 12 hours, and the product was filtered, and the unreacted 1-allyl-3-methylimidazolium chloride was removed by washing with deionized water for several times, and finally, it was repeatedly washed with deionized water for three times, and then ion exchange was completed by soaking in 15% sodium sulfate at 70°C for 20 hours, and the product was washed with deionized water; finally, it was dried at 60°C to obtain a perfluoro amphoteric ion exchange resin, which was recorded as A4, and the reaction formula is as follows:
[0109]
[0110] The product A4 ( Figure 1 , D) Infrared transmission spectrum measurement, it can be seen that in the range of 3304-3400cm -1 and 1548 cm -1 The characteristic peak (-NH2 group) belonging to the primary amine -SO2NH2 disappears, and at 3300cm -1 The characteristic peak of -NH- appeared near 3038~3110cm -1 The absorption peak of CH (attributed to -CH2 and -CH3 on the imidazole ring) appeared at 1573 cm -1 There is a strong characteristic absorption peak at 1060 cm -1 -SO3 - The characteristic peaks of the above positions are assigned to references Journal of Membrane Science 362 (2010) 97-104, Journal of Membrane Science 515 (2016): 268-276. The above results prove that the target product is successfully obtained.
[0111] After ion exchange capacity (IEC) measurement, the IEC of the obtained target product A4 is 1.11 mmol / g, and in the structure of the obtained target product A4, a+b / (a+b+c+d)=0.73; c+d / (a+b+c+d)=0.27.
[0112] The overall molar fraction of tetrafluoroethylene polymerization units in the copolymer is 48.00%, the overall molar fraction of perfluoro anion units is 38.20%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 13.80%.
[0113] Embodiment 5:
[0114] A perfluoro amphoteric ion exchange resin is prepared. First, the target resin is synthesized according to the method of Example 4, except that a′=3, b′=1; x, z=1, y=0 in the PFSO2F resin, the number average molecular weight is 430,000, and the molar equivalent E w =689 g / mol), the resin was immersed in a 25wt% sulfuric acid solution at 70°C for 24h to complete ion exchange, and the -SO3Na in the anion structural unit was converted into -SO3H to obtain a perfluoro amphoteric ion exchange resin, denoted as A5, and the obtained product structure is as follows:
[0115]
[0116] After ion exchange capacity (IEC) measurement, the IEC of the anion structural unit of the obtained target product A5 is 1.45 mmol / g, and in the structure of the obtained target product A5, a+b / (a+b+c+d)=0.64; c+d / (a+b+c+d)=0.36.
[0117] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 46.20%, the overall molar fraction of perfluoro anion units is 35.20%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 18.60%.
[0118] Embodiment 6:
[0119] A perfluoro amphoteric ion exchange resin is prepared by first preparing an intermediate product according to the method of Example 3, except that the PFSO2F resin (E w =689g) and NH3 with NH3 The reaction time was extended from 120min to 200min, and the other components, material ratios and synthesis methods were the same as those in Example 3. The structure of the intermediate product was the same as that of A3, except that b / (a+b+c+d)=0.32; d / (a+b+c+d)=0.25 in the structure, and the IEC of the obtained resin anion structural unit was 1.43mmol / g.
[0120] 10g of the obtained product was added to 200mL of dry N,N-dimethylacetamide, the stirring device was turned on, and it was slowly heated to 80°C. After it was completely dissolved, 0.03g of 1-allyl-3-methylimidazolium chloride was added. The molar ratio of the intermediate product to 2,3-epoxypropyltrimethylammonium chloride (Q-Ar reagent) was about 1:8. After the addition was completed, -SO2NH2 was used to react with the epoxy group to graft the cationic group under mechanical stirring at 80°C. The obtained product was finally immersed in 15% lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) at 70°C for 20h to complete ion exchange, and the counter ion in the cationic group was converted into [(CF3SO2)2N] - , abbreviated as TFSI - , a perfluoro amphoteric ion exchange resin was obtained, denoted as A6, in which a+b / (a+b+c+d)=0.56; c+d / (a+b+c+d)=0.44, and the IEC of the obtained resin was 1.40 mmol / g.
[0121] The reaction formula is as follows:
[0122]
[0123] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 48.50%, the overall molar fraction of perfluoro anion units is 36.10%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 15.40%.
[0124] Embodiment 7:
[0125] A preparation method of a perfluoroamphoteric exchange resin, comprising the following steps:
[0126] The target product A5 prepared in Example 5 was treated with a 20% phosphoric acid solution for 24 hours to complete ion exchange, and a perfluoroamphoteric ion exchange resin was obtained, which was recorded as A7. The IEC of the anion structural unit was 1.42 mmol / g, and a+b / (a+b+c+d)=0.64; c+d / (a+b+c+d)=0.36 in the structure. The structure of the obtained product is as follows:
[0127]
[0128] The overall molar fraction of tetrafluoroethylene polymer units in the copolymer is 48.40%, the overall molar fraction of perfluoro anion units is 35.20%, and the overall molar fraction of perfluoro perfluoro cationic structural units is 16.40%.
[0129] Embodiment 8:
[0130] A method for preparing a homogeneous perfluorinated zwitterionic membrane comprises the following specific steps:
[0131] First, the PFSO2F resin was immersed in a 15% KOH solution at 60°C for 48 hours to convert all -SO2F groups into -SO3K, and then washed with deionized water; dried at 60°C for 24 hours to obtain a perfluoro anion resin (same structure as A1, except that d=0 in the structural unit), denoted as A8, with an IEC of 0.97mmol / g. Secondly, the mixed resin (A8 molar content of 70.00%; A1 molar content of 30.00%) was dissolved in N,N-dimethylformamide, and a 10wt% homogeneous perfluoro amphoteric resin solution was prepared after stirring and dispersing evenly, and coated on a polytetrafluoroethylene reinforced mesh (2 layers, porosity of 80%, gram weight of 3.2g / m 2 ), pre-dried at 80°C, placed in an oven at 145°C for 90 minutes, taken out and demolded, to prepare a 15 μm homogeneous perfluoro zwitterionic membrane (the molar content of the perfluoro anion structural unit is 94.0%, and the molar content of the perfluoro cation structural unit is 6.0%), and the IEC is 0.95 mmol / g.
[0132] Embodiment 9:
[0133] A method for preparing a homogeneous perfluoro zwitterionic membrane, the preparation process is referred to Example 8, except that the obtained ion membrane is immersed in 25wt% sulfuric acid at 60°C for 20h to complete ion exchange, converting all -SO3K into perfluorosulfonic acid groups -SO3H, and at the same time converting the counter ion in the cationic group into -HSO4 - The product was washed with deionized water and dried at 60°C for 30 h to obtain a 15 μm homogeneous perfluorozwitterionic membrane (the molar content of the perfluoroanionic structural unit was 95.5%, and the molar content of the perfluorocationic structural unit was 4.5%) with an IEC of 0.96 mmol / g.
[0134] Embodiment 10:
[0135] A method for preparing a homogeneous perfluoro zwitterionic membrane, the preparation process is referred to Example 8, except that the molar content of A8 in the mixed resin accounts for 60.0%, and the molar content of A4 accounts for 40.0%. The mixed resin is dissolved in N, N-dimethylacetamide, stirred and dispersed evenly to prepare a 10wt% homogeneous perfluoro zwitterionic resin solution, which is coated on a polyvinylidene fluoride reinforced mesh (3 layers, porosity 80%, gram weight 3.2g / m 2 ), pre-dried at 80°C, placed in an oven at 145°C for 90 minutes, removed from the mold, and soaked in 20wt% sulfuric acid at 60°C for 22 hours to complete ion exchange, converting all -SO3Na into perfluorosulfonic acid groups -SO3H, and at the same time converting the counter ions in the cationic groups into -HSO4 -The product was washed with deionized water and dried at 60°C for 30 h to obtain a 13 μm homogeneous perfluorozwitterionic membrane (the molar content of the perfluoroanionic structural unit was 88.7%, and the molar content of the perfluorocationic structural unit was 11.3%) with an IEC of 0.96 mmol / g.
[0136] Embodiment 11:
[0137] A method for preparing a homogeneous perfluoro zwitterionic membrane comprises dissolving resin A4 (all perfluoro zwitterionic ion exchange resins are used in the mixed resin) in isopropanol, stirring and dispersing the resin to prepare a 16 wt% perfluoro zwitterionic resin solution, and then pouring the solution on a polypropylene reinforced mesh (3 layers, porosity of 82%, gram weight of 2.9 g / m 2 ), pre-dried at 80°C, placed in an oven at 145°C for 90 minutes, removed from the mold, and immersed in 20wt% sulfuric acid at 60°C for 22h to complete ion exchange, converting all -SO3Na into perfluorosulfonic acid groups -SO3H, and preparing an 18μm homogeneous perfluoro amphoteric ion exchange tree membrane (the molar content of perfluoro anion structural units is 69.5%, and the molar content of perfluoro cation structural units is 31.5%), with an IEC of 1.14mmol / g.
[0138] Embodiment 12:
[0139] A method for preparing a homogeneous perfluoro zwitterionic membrane, wherein the ion exchange is completed after the ion membrane prepared in Example 11 is treated with a 20% phosphoric acid solution for 24 hours, and the counter ion in the cationic group is ionized to -H2PO4 - , a 18 μm homogeneous perfluorozwitterionic ion exchange membrane was obtained (the molar content of the perfluoro anion structural unit was 71.0%, and the molar content of the perfluoro cation structural unit was 29.0%), and the IEC was 1.10 mmol / g.
[0140] Embodiment 13:
[0141] A method for preparing a heterogeneous perfluoro zwitterionic membrane, wherein the PFSO2F resin in Example 1 is selected and melt-extruded into a film by a twin-screw extruder at 260°C to prepare a polymer base membrane. According to method (1), a reaction is carried out on the surface of the base membrane to synthesize a perfluoro zwitterionic polymer structure. The specific implementation method is as follows: the base membrane is immersed in a triethylamine solution, wherein the molar ratio of PFSO2F to TEA is about 1:5; then the base membrane is reacted at 60°C and mechanically stirred for 0.5h and then cooled to room temperature. After the reaction is completed, the -SO2F group on the surface of the base membrane is partially converted into -SO2Et3N, the product is filtered, and the excess triethylamine is washed with deionized water; finally, it is dried at 60°C to obtain an intermediate product. Finally, the intermediate product was immersed in a 15% KOH solution at 60°C for 24h to completely convert the counter ions in the cationic group into hydroxide ions, and the remaining -SO2F in the base membrane was converted into -SO3K. The product was washed with excess alkali solution with deionized water; finally, it was dried at 60°C to obtain a heterogeneous perfluorozwitterionic membrane (the molar content of perfluoroanionic structural units was 92.8%, and the molar content of perfluorocationic structural units was 7.2%), and the zwitterionic structural units were successfully constructed on the membrane surface, and their structure was the same as A1, and the IEC was 0.90mmol / g.
[0142] Embodiment 14:
[0143] A method for preparing a heterogeneous perfluoro zwitterionic membrane comprises selecting the PFSO2F resin in Example 1 and performing melt extrusion at 300°C through a twin-screw extruder to form a polymer base membrane. First, according to the method in Example (3), the PFSO2F base membrane is reacted with ammonia to convert the -SO2F groups on the surface of the base membrane into -SO2NH2, and then reacting according to method (2) to graft the cationic groups. The grafting process is referred to Example 4.
[0144] The excess ammonia was washed with deionized water and finally dried at 60°C to obtain the intermediate product. Finally, the intermediate product was immersed in a 15% KOH solution at 60°C for 24 hours to completely convert the counter ions in the cationic groups into OH - At the same time, the remaining -SO2F in the base membrane is converted into -SO3K, and the product is washed with deionized water to remove excess alkali solution; finally, it is dried at 60°C to obtain a heterogeneous perfluorinated zwitterionic membrane (the molar content of the perfluorinated anion structural unit is 93.0%, and the molar content of the perfluorinated cation structural unit is 7.0%). The zwitterionic structural unit is successfully constructed on the membrane surface, and its structure is the same as A4 (the cationic group is OH - ), IEC is 0.89mmol / g.
[0145] Comparative Example 1
[0146] The PFSO2F resin in Example 1 was selected and immersed in 15% KOH and 25wt% sulfuric acid solutions at 80°C for 30h to complete ion exchange, and all -SO2F groups were converted into -SO3H to obtain a perfluoro anion resin, i.e., a perfluorosulfonic acid resin PFSA, with an IEC of 1.00mmol / g.
[0147] Comparative Example 2
[0148] The PFSO2F resin and TEA are reacted according to step (1) in Example 1, except that the molar ratio of the PFSO2F resin to TEA is about 1:10; after the addition is completed, the reaction is carried out at 60° C. and mechanically stirred for 30 hours, and then all the -SO2F groups are grafted with cationic groups to convert into -SO2Et3N to obtain a perfluorocationic resin, i.e., a perfluoroquaternary amine resin PFSN, with an IEC of 0.90 mmol / g.
[0149] Comparative Example 3
[0150] Referring to Example 8, the mixed resin (A8 molar content of 94.00%; PFSN molar content of 6.00%) was dissolved in N, N-dimethylformamide, stirred and dispersed evenly to prepare a 10wt% homogeneous perfluoroampholytic resin solution, which was coated on a polytetrafluoroethylene reinforced mesh (2 layers, porosity of 80%, gram weight of 3.2g / m 2 ), pre-dried at 80°C, placed in an oven at 145°C for 90 minutes, taken out and demolded, to prepare a 15 μm homogeneous perfluoro zwitterionic membrane (the molar content of the perfluoro anion structural unit is 94.0%, and the molar content of the perfluoro cation structural unit is 6.0%), and the IEC is 0.95 mmol / g.
[0151] Comparative Example 4
[0152] The perfluorosulfonic acid resin PFSA obtained in Comparative Example 1 was selected to prepare a perfluorosulfonic acid proton exchange membrane according to the steps of Example 2, and the IEC was 0.96 mmol / g.
[0153] Comparative Example 5
[0154] The perfluoro quaternary amine resin PFSN obtained in Comparative Example 2 was selected to prepare a perfluoro anion exchange membrane according to the steps of Example 2, and the IEC was 0.88 mmol / g.
[0155] Comparative Example 6
[0156] DuPont's perfluorosulfonic acid proton exchange membrane model NRE211 has an IEC of 0.90 mmol / g.
[0157] Comparative Example 7
[0158] A201 anion exchange membrane from Tokuyama Company of Japan, IEC is 1.70mmol / g.
[0159] Table 1 is the performance data of perfluoroampholytic exchange resin and comparative examples 1-2
[0160]
[0161]
[0162] As can be seen from the above table, after being tested by the Fenton test for 200 hours, the IEC is all above 90%, and the thermal degradation temperature is all above 330°C. Compared with the perfluorosulfonic acid resin PFSA and the perfluoroquaternary amine resin PFSN, the perfluoroamphoteric exchange resin prepared by the present invention has high chemical stability, high thermal stability, and high IEC; in addition, since the cationic structure introduced into the resin structure can form an ion pair with the anionic structural unit (acid-base ion pairs are formed between positive and negative charges), the interaction force between the two units is enhanced, the degradation of the polymer is weakened or slowed down, the chemical stability and thermal stability of the resin are improved, and the water absorption rate of the resin is effectively limited (less than 30%).
[0163] Table 2 is the performance data of perfluoro zwitterionic membrane and comparative examples 3-6
[0164]
[0165]
[0166] As can be seen from the above table, the zwitterionic membrane disclosed in the embodiment of the present invention has more excellent mechanical properties, dimensional stability and lower vanadium ion permeation than the ion membrane in the prior art. In addition, the ionic conductivity of the ion membrane at high temperature and room temperature can be improved by regulating the structure of the cation and anion groups, and the vanadium resistance performance of the ion membrane can be improved while maintaining the conductivity and mechanical properties of the ion membrane, which can improve the shortcomings of the ion membrane with poor vanadium resistance performance and low high temperature conductivity.
Claims
1. A perfluoro amphoteric ion exchange resin, characterized in that: The resin structure contains both perfluorinated anion structural units and perfluorinated cation structural units, and the resin has a structure shown in the following formula I: Wherein ad is an integer from 0 to 30, and x is 0 or 1; y, z are integers of 0 to 3, e is 50 to 10000; a+b / (a+b+c+d)=0.05 to 0.9; c+d / (a+b+c+d)=0.1 to 0.95; in the perfluoroanion structural unit, M is H + , Li + 、Na + , K + 、Ag + NH4 + NH3 + Mg 2+ 、Al 3+ , Ca 2+ , Ba 2+ , Fe 2+ , Fe 3+ , Cu 2+ 、Zn 2+ , Mn 2+ One of the following; the cationic group Ar1 structure in the B unit contains one or more The counter ion Ar2 in the perfluorocation structural unit is Cl - ,Br - , I - , F - , NO3 - , OH - , HCO3 - ,CO3 2- , CH3COO - , SCN - , SO4 2- , HSO3 - , HSO4 - , ClO4 - , S2O3 2- , C2O4 2- , HSO4 - , PF6 - , BF4 - , [C(CN)3] - , [(FSO2)2N] - , [(CF3SO2)2N] - , [B(CN)4] - , [(C2F5)3PF3] - , (H2PO4) - , (H2PO3) - , [(H2PO4) - (H3PO4) n , n>1],(H2PO4) - , HSO3 - , SO3 - One of them.
2. The perfluoro amphoteric ion exchange resin according to claim 1, characterized in that a, c are 1 to 10; b, d = 1; x = 1; y, z = 0, 1; a + b / (a + b + c + d) = 0.15 ~ 0.65; c + d / (a + b + c + d) = 0.35 ~ 0.85; in the perfluoro anion structural unit, M is H + , K + , Li + , NH4 + One of the following; the structure of the cationic group Ar1 in the perfluorocation structural unit is shown in Formula II: Ar2 is Cl - , OH - , [(CF3SO2)2N] - , (H2PO3) - , [(H2PO4) - (H3PO4) n , n>1].
3. The perfluoro amphoteric ion exchange resin according to claim 1, characterized in that The cationic group structure is selected from one of Formula III:
4. The perfluoro amphoteric ion exchange resin according to claim 1, characterized in that The ion exchange capacity of the resin is 0.5 to 2.5 mmol / g.
5. The perfluoro amphoteric ion exchange resin according to claim 1, characterized in that The ion exchange capacity of the resin is 0.9 to 1.6 mmol / g.
6. The method for preparing the perfluoro amphoteric ion exchange resin according to any one of claims 1 to 5, characterized in that: Choose one of the following methods: Method 1: (1-1) A perfluorovinyl ether sulfonyl fluoride resin is subjected to a one-step grafting reaction with an Ar reagent having a tertiary amine or tertiary phosphorus group in an organic solvent to graft a cationic group to synthesize an intermediate product; or, PFSO2F is first pre-swollen in an organic solvent, and then subjected to a grafting reaction with an Ar reagent to graft a cationic group to synthesize an intermediate product; (1-2) subjecting the obtained intermediate product to ion exchange through a post-treatment process of alkali, acid, or salt containing M ions, converting the unreacted sulfonyl fluoride group -SO2F into a perfluorosulfonic acid group -SO3M, and washing and drying to obtain a perfluoro amphoteric ion exchange resin; Method 2: PFSO2F is pre-swelled in an organic solvent and reacted with ammonia, with a molar ratio of resin to ammonia of 1:15; part of the -SO2F groups are converted into -SO2NH2, and after the reaction, the remaining -SO2F groups are converted into -SO3H through an acid-base treatment process, thereby obtaining a structural unit containing both -SO3H and -SO2NH2, thereby forming -SO3 - HN + HSO2-acid-base ion pair, after washing and drying, amphoteric ion exchange resin is obtained; or PFSO2F is pre-swollen in an organic solvent and reacted with ammonia, and the molar ratio of resin to ammonia is 1:15; part of the -SO2F group is converted into -SO2NH2 to obtain an intermediate product, and then the intermediate product is grafted with a Q-Ar reagent with a cationic group in an organic solvent for grafting the cationic group, and finally the remaining -SO2F group is converted into -SO3M through an acid, base and salt ion exchange process, and the amphoteric ion exchange resin is obtained after washing and drying.
7. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: The Ar reagent is a reagent containing one or more tertiary amines or tertiary phosphorus structures, and its general structural formula is shown in Formula IV:
8. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: The structure of the Ar reagent is one of the structures shown in Formula V:
9. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: The Q-Ar reagent is a reagent with one or more quaternary amine or quaternary phosphonium structures, and its general structural formula is shown in Formula VI, wherein at least one of R1 to R4 is a cationic group containing one or more, and the structure of the cationic group is shown in Formula II; the remaining substituent groups in the structure are -F, -Cl, -H, -Br, -OH, -C H3 、-OC H3 , -Ph, -OPh, -CH2Cl, -CH2Br, -CH2CH3; 10. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: The structure of the Q-Ar reagent is one of the structures shown in Formula VII:
11. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: The organic solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, ethanol, isopropanol, dimethyl sulfoxide or ethyl acetate; In method 1, the molar ratio of the perfluorosulfonyl fluoride resin to the monomer reagent of the Ar reagent is 1:5-20; in method 2, the molar ratio of the intermediate product to the monomer reagent of the Q-Ar reagent is 1:3-20; In methods 1 and 2, the mass volume ratio of PFSO2F resin to organic solvent is 1:1-12 g / mL; The grafting reaction temperature is 15 to 150° C., and the grafting reaction time is 1 to 48 hours; The pre-swelling in method 1 is to swell the perfluorosulfonyl fluoride resin in an organic solvent at 40 to 50° C. for 60 to 300 minutes.
12. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: In methods 1 and 2, the mass volume ratio of PFSO2F resin to organic solvent is 1:1-6 g / mL; the temperature of the grafting reaction is 25-80° C., and the time of the grafting reaction is 5-12 hours.
13. The method for preparing the perfluoro amphoteric ion exchange resin according to claim 6, characterized in that: In the acid, base and salt ion exchange process, the base is one of sodium hydroxide, triethylamine, trimethylamine, ammonia water and potassium hydroxide, and the concentration is 5-50wt%; the acid is one of hydrochloric acid, phosphoric acid, sulfuric acid, acetic acid and nitric acid, and the concentration is 5-50wt%; the salt is one of potassium chloride, lithium hexafluorophosphate, lithium hypochlorite, lithium tetrafluoroborate, lithium bistrifluoromethanesulfonyl imide, ammonium chloride, sodium sulfate, ammonium sulfate, ammonium carbonate, ammonium nitrate, sodium phosphate and sodium nitrate, and the concentration is 5-50wt%.
14. A perfluorinated zwitterionic ion exchange membrane, characterized in that: The ion membrane structure contains the perfluoroamphoteric ion exchange resin component according to any one of claims 1 to 5 or the perfluoroamphoteric ion exchange resin component prepared by the method according to any one of claims 6 to 13, wherein the molar content percentage of the perfluoroamphoteric ion exchange resin in the membrane is 1 to 100%.
15. The perfluorozwitterionic ion exchange membrane according to claim 14, characterized in that: The thickness of the perfluoro amphoteric ion exchange membrane is 5 to 250 μm, and the thermal degradation temperature is 255 to 350° C.
Citation Information
Patent Citations
Preparation method of water retention type proton exchange membrane for fuel cell
CN101667648A
Modified inorganic nanoparticles, polymer mixed slurry, composite membrane and preparation method
CN111100328A
Preparation method of perfluorosulfonic acid membrane with adjustable microstructure
CN111370723A
Polymerization method of perfluorosulfonyl fluoride resin
CN114835842A
Preparation method of perfluorinated sulfonamide-based anion exchange membrane
CN104710639A