A particle-free copper conductive ink and conductive copper film for 3D inkjet printing and a preparation method thereof
By using particle-free copper conductive ink composed of copper tetrahydrate, complexing agent and additive, the problems of easy oxidation and poor stability of nano-copper-based ink are solved, and high stability and conductivity in 3D inkjet printing are achieved , suitable for 3D inkjet printing and the preparation of conductive copper films.
Patent Information
- Application Number
- CN202310246986.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-14
AI Technical Summary
The existing nano-copper-based conductive inks are prone to oxidation, have poor conductivity and poor stability during storage, resulting in particle settlement and agglomeration problems in 3D inkjet printing, limiting its application.
None composed of copper formate tetrahydrate, complexing agents (such as 1,2-propylene diamine and n-octylamine) and additives (such as sodium dodecylbenzenesulfonate and cetyltrimethylammonium bromide) Particulate copper conductive ink, by adjusting component ratio and process steps, a particulate copper conductive ink with moderate viscosity is prepared to ensure high storage stability and be suitable for 3D inkjet printing.
Achieve long-term storage stability of particle-free copper conductive ink, avoid particle precipitation, ensure pattern accuracy and conductive performance of 3D inkjet printing, suitable for printing lines and patterns on non-planar substrates, and reduce during sintering. The size difference is reduced, and the uniformity and conductivity of the conductive copper film are improved.
Smart Images

Figure CN116285503B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of conductive ink, and in particular to a particle-free copper conductive ink and a conductive copper film for 3D inkjet printing and a preparation method thereof. Background Art
[0002] Printed electronics technology has the characteristics of low cost, low energy consumption, green environmental protection, and the ability to achieve large-area, personalized, and flexible manufacturing. Printed electronics is to transfer functional inks onto the surface of the substrate and give it the required electrical properties through certain post-processing. A key factor restricting the development of printed electronics technology is the preparation of conductive inks. At present, 3D inkjet printing technology is based on the working principle of inkjet printers. Under the stimulation of digital signals, the liquid in the nozzle chamber forms droplets in an instant, and is ejected from the nozzle at a certain speed and frequency. It is solidified layer by layer along the specified path to finally obtain a 3D solid.
[0003] Since most conductive inks suitable for inkjet printing are based on gold and silver, which are relatively expensive metals, researchers have also chosen copper, which has advantages such as low price and high conductivity, to replace gold and silver. However, nano copper-based conductive inks have the disadvantages of being easily oxidized, having poor conductivity and poor stability. The copper conductive ink of the general nanoparticle system is very prone to sedimentation, agglomeration and oxidation during storage. Even if a surfactant is added for protection, its shelf life does not exceed two weeks. The sedimentation and agglomeration of particles can be observed with the naked eye. Copper particles with a particle size of 20nm agglomerated into large particles with an average particle size of 40μm after two weeks. For 3D inkjet printing nozzles, copper particles of this particle size will definitely clog the nozzles, which has application difficulties in 3D inkjet printing and limits the further development of copper-based conductive inks. Summary of the invention
[0004] The present invention provides a particle-free copper conductive ink and a conductive copper film for 3D inkjet printing and a preparation method thereof, so as to provide a particle-free copper conductive ink with moderate viscosity, high ink storage stability, no particle precipitation during long-term storage, and meet the precision requirements of 3D inkjet printing technology.
[0005] In order to solve the above technical problems, one of the purposes of the present invention is to provide a particle-free copper conductive ink for 3D inkjet printing, comprising the following components by mass fraction:
[0006] Copper formate tetrahydrate: 25wt%-45wt%;
[0007] Complexing agent: 35wt%-45wt%;
[0008] Additives: 4wt%-6wt%;
[0009] Solvent: balance;
[0010] Wherein, the complexing agent is 1,2-propylenediamine and / or n-octylamine; the auxiliary agent is sodium dodecylbenzenesulfonate and / or hexadecyltrimethylammonium bromide; and the solvent is ethanol and / or methanol.
[0011] By adopting the above scheme, the copper-based conductive ink involved in this application is composed of copper formate tetrahydrate, solvent, chelating agent and auxiliary agent, and the color is dark blue. The chelating agent and auxiliary agent components used in this application are added to the copper formate tetrahydrate system, do not contain any particulate matter, have high storage stability, can be used for 3D inkjet printing technology, and are printed into lines or patterns on non-planar substrates. The added auxiliary agent helps to reduce the size difference during the sintering process of the conductive copper film, promotes uniform particle distribution, and avoids uneven nucleation during the sintering process to produce copper particles of different sizes. In addition, the addition of auxiliary agents can adjust the hydrophilic angle between the ink and the 3D printing substrate, which is convenient for 3D printing on different substrate materials to prepare lines and patterns with sufficient precision. The ink has high storage stability and no particle precipitation occurs during long-term storage, which is helpful for application in the field of 3D inkjet printing.
[0012] As a preferred embodiment, the complexing agent includes 1,2-propylenediamine and n-octylamine in a mass ratio of (1-3):(1-3).
[0013] By adopting the above scheme, diamine substances have better complexing ability than monoamine substances, and can react with copper formate tetrahydrate to form a copper complex with high solubility. As for the viscosity of the ink, when the viscosity of the ink is too high, it will cause the ink droplets to be generated and ejected, and it will be impossible to print. If the viscosity is too low, the ink will spread easily on the surface of the substrate after printing, resulting in a decrease in the accuracy of the printed pattern and affecting the quality of the conductive circuit. Under the premise of ensuring a higher conductivity, the present application controls the viscosity of the particle-free copper conductive ink by adjusting the type and content of the solvent and the additive to achieve a preferred viscosity range of 15-20mPa·s to meet the requirements of 3D inkjet printing pattern accuracy.
[0014] As a preferred embodiment, the auxiliary agent is sodium dodecylbenzenesulfonate and hexadecyltrimethylammonium bromide in a mass ratio of 1:1.
[0015] As a preferred embodiment, the solvent is ethanol and / or methanol.
[0016] In order to solve the above technical problems, the second object of the present invention is to provide a method for preparing a particle-free copper conductive ink for 3D inkjet printing, comprising the following steps:
[0017] (1) weighing each component according to the component ratio, mixing the complexing agent and the solvent, adding an auxiliary agent, stirring and mixing uniformly to obtain a mixed solution;
[0018] (2) copper formate tetrahydrate is added to the mixed solution, stirred in a closed container until completely dissolved, and filtered through a microporous filter membrane to obtain a particle-free copper conductive ink.
[0019] As a preferred embodiment, in step (1), the mixing time is 0.5h-5h; in step (2), the stirring time is 5h-10h; and filtering is performed sequentially using microporous filter membranes with pore sizes of 450nm and 220nm.
[0020] In order to solve the above technical problems, the third object of the present invention provides a conductive copper film, which is prepared by 3D inkjet printing using particle-free copper conductive ink.
[0021] In order to solve the above technical problems, the fourth object of the present invention provides a method for preparing a conductive copper film, comprising the following steps: printing particle-free copper conductive ink on a flexible substrate by a microelectronic inkjet printer, and sintering it in an inert gas or reducing gas atmosphere to obtain a conductive copper film.
[0022] As a preferred solution, the sintering temperature is 150°C-300°C, and the sintering time is 1 min-15 min.
[0023] As a preferred solution, the flexible substrate is cyanate, polyethylene terephthalate or a quartz sheet.
[0024] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0025] 1. The copper-based conductive ink involved in the present invention does not contain any particles. The complexing agent and auxiliary agent components of the present application are added to the copper formate tetrahydrate system, have high long-term storage stability, and can be used for 3D inkjet printing technology to print lines or patterns on non-planar substrates. The auxiliary agent helps to reduce size differences during the sintering process of preparing conductive copper films, promotes uniform distribution of particles, and can also adjust the hydrophilic angle between the ink and the 3D printing substrate, which is convenient for 3D printing of lines and patterns with sufficient precision on different substrate materials.
[0026] 2. Compared with monoamines, diamines have better complexing ability and can react with copper formate tetrahydrate to form copper complexes with high solubility. Under the premise of ensuring high conductivity, the present application adjusts the viscosity of the particle-free copper conductive ink by adjusting the type and content of solvents and additives to achieve a preferred viscosity range of 16-20 mPa·s to meet the requirements of 3D inkjet printing pattern accuracy and avoid nozzle clogging due to excessive viscosity or affecting 3D printing accuracy due to too low viscosity.
[0027] 3. Since copper is easily oxidized in the air, the conductive copper film of the present application is sintered and heat-treated in an inert gas or reducing gas environment to obtain a conductive copper film, which has broad application prospects in printed electronics. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : is an XRD diagram of a particle-free copper conductive ink in Example 4 of the present invention;
[0029] Figure 2 : A SEM image of a conductive copper film prepared from a particle-free copper conductive ink in Example 5 of the present invention;
[0030] Figure 3 : This is a SEM image of a conductive copper film prepared by a particle-free copper conductive ink in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Examples 1-7 and Comparative Examples 1-3
[0033] A copper conductive ink, as shown in Table 1 below, includes a copper precursor, a solvent, a chelating agent and an auxiliary agent, wherein the copper precursor is copper formate tetrahydrate or copper oxide, the chelating agent is 1,2-propylenediamine and / or n-octylamine, the auxiliary agent is at least one of sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium bromide and sodium dodecyl sulfate, and the solvent is anhydrous ethanol.
[0034] The above-mentioned method for preparing the copper conductive ink comprises the following steps:
[0035] (1) Weighing each component according to the component ratio, mixing the complexing agent with anhydrous ethanol, adding an auxiliary agent, and mixing uniformly by magnetic stirring for 2 hours to obtain a mixed solution;
[0036] (2) copper formate tetrahydrate was added to the mixed solution, and the mixture was stirred by magnetic force for 5 hours in a closed beaker until it was completely dissolved, and filtered sequentially with microporous filter membranes with pore sizes of 450 nm and 220 nm to obtain a particle-free conductive ink that can be heated in nitrogen to prepare a conductive pattern.
[0037] The method of using the above-mentioned particle-free conductive ink for preparing a conductive pattern by heating in nitrogen is as follows: the copper conductive ink prepared in the embodiment is a particle-free ink, which is dark blue. The particle-free conductive ink is 3D printed on a tile-shaped cyanate substrate by a microelectronic inkjet printer, and sintered in a nitrogen atmosphere. The sintering conditions are: heating to 180°C, and the sintering time is 5 minutes to obtain a conductive copper film bonded to the tile-shaped cyanate substrate.
[0038] Table 1 - Components and contents in Examples 1-7 and Comparative Examples 1-3 of the present application
[0039]
[0040]
[0041] Performance testing
[0042] 1. Ink viscosity: Anton Paar model ViscoQC 300R viscometer was used to test the ink viscosity of the embodiment and the comparative example. The ink viscosity requirement for 3D inkjet printing is 1-22 mPa·s, and more preferably 16-20 mPa·s. The results are shown in Table 2 below.
[0043] 2. Resistivity of conductive copper film: The resistivity of the conductive copper films prepared in the embodiment and the comparative example was tested using a FT-346 four-probe resistance tester from Ruike Instrument Co., Ltd. The test results are shown in Table 2 below.
[0044] 3. Contact angle: The contact angle of the conductive ink on the surface of the cyanate substrate is measured by an OCA35 video optical contact angle meter. The contact angle is automatically calculated by taking photos and using software. The larger the contact angle, the higher the accuracy of the circuit prepared by inkjet printing; the smaller the contact angle, the easier it is for the ink to spread on the substrate during printing, seriously affecting the printing accuracy. The preferred contact angle in this application is greater than 55°.
[0045] 4. Particle size and stability detection: The particle size of the ink of the embodiment and the comparative example was detected by a Malvern laser particle size analyzer. The minimum particle size detected was 0.3 nm. If the particle size could not be measured, it was proved to be a particle-free type. The stability test was to store the ink in a dense and light-proof environment for 4 months and detect the change in particle size after 4 months. The results are shown in Table 2 below.
[0046] Table 2 - Performance test results of the present application examples and comparative examples
[0047]
[0048]
[0049] Combining the performance test results of Examples 1 and 6 and Comparative Examples 1 and 3 in Table 2, it can be seen that compared with sodium dodecyl sulfate, the present application adds hexadecyltrimethylammonium bromide or sodium dodecylbenzenesulfonate, which helps to reduce size differences and promote uniform particle distribution during the sintering process of preparing a conductive copper film when lines or patterns are printed on a non-planar substrate using 3D inkjet printing technology. At the same time, it can increase the contact angle between the ink and the 3D printed substrate, adjust the viscosity, and facilitate 3D printing on different substrate materials. Prepare lines and patterns with sufficient precision, and at the same time, have high storage stability and no particles are generated.
[0050] Combining the performance test results of Example 1 and Comparative Example 2 in Table 2, it can be seen that the copper-based conductive ink involved in the present application uses copper formate tetrahydrate as a precursor, and the prepared ink does not contain any particulate matter. The complexing agent and auxiliary agent components are added to the copper formate tetrahydrate system, which can ensure that the ink has high long-term storage stability and no particles are generated. When used in 3D inkjet printing technology, the particle-free requirement is met. The addition of auxiliary agents can also inhibit the coarsening of copper elemental particles during subsequent ink sintering, thereby achieving the purpose of reducing resistance.
[0051] Combining the performance test results of Examples 1 and 4-5 in Table 2, it can be seen that since diamine substances have better complexing ability than monoamine substances, they can react with copper formate tetrahydrate to form a copper complex with high solubility. Under the premise of ensuring high conductivity, the present application simultaneously adds n-octylamine and 1,2-propylenediamine to adjust the viscosity of the particle-free copper conductive ink to achieve a preferred viscosity range of 16-20 mPa·s, so as to meet the requirements of 3D inkjet printing pattern accuracy and avoid nozzle clogging caused by excessive viscosity or 3D printing accuracy affected by too low viscosity.
[0052] 5. The X'pert Powder multi-position automatic sampling X-ray diffractometer produced by PANalytical of the Netherlands was used to test the film phase. The XRD spectrum of the conductive copper film obtained in Example 4 is as follows: Figure 1 The morphology of the conductive copper film was observed using a Quanta200 environmental scanning electron microscope. The SEM image of the conductive copper film obtained in Example 5 is shown in FIG. Figure 2 As shown, the SEM image of the conductive copper mold prepared in Comparative Example 1 is as follows Figure 3 shown.
[0053] like Figure 2 As shown, after the surfactant is added to Example 5, the abnormal growth of copper particles will be suppressed during sintering reduction, and the copper particles formed will be uniform in size, which is conducive to uniform distribution. More sintering necks will be formed during sintering to form a film, which will improve the conductive performance. At the same time, the surface roughness of the macroscopic copper film formed is reduced, which is conducive to obtaining a conductive pattern with high smoothness and strong conductive performance.
[0054] like Figure 3As shown, when no surfactant is added to Comparative Example 1, larger copper particles will be produced during sintering reduction, which is not conducive to uniform distribution. The sintering necks formed at the microscopic level are reduced, resulting in a decrease in conductivity. A large number of micropores exist in the formed macroscopic copper film, and the surface roughness of the copper film is increased, which is not conducive to obtaining a copper film with high surface finish and strong conductivity.
[0055] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.
Claims
1. A particle-free copper conductive ink for 3D inkjet printing, characterized in that: The following components are included in mass fraction: Copper formate tetrahydrate: 25wt%-45wt%; Complexing agent: 35wt%-45wt%; Additives: 4wt%-6wt%; Solvent: balance; Among them, when the complexing agent is 1,2-propylenediamine, the auxiliary agent is hexadecyltrimethylammonium bromide; when the complexing agent is 1,2-propylenediamine and n-octylamine in a mass ratio of 1:1, the auxiliary agent is sodium dodecylbenzenesulfonate and hexadecyltrimethylammonium bromide in a mass ratio of 1:1 or a single hexadecyltrimethylammonium bromide.
2. A particle-free copper conductive ink for 3D inkjet printing according to claim 1, characterized in that: The solvent is ethanol and / or methanol.
3. A method for preparing a particle-free copper conductive ink for 3D inkjet printing based on claim 1 or 2, characterized in that: The following steps are involved: (1) weighing each component according to the component ratio, mixing the complexing agent and the solvent, adding an auxiliary agent, stirring and mixing uniformly to obtain a mixed solution; (2) copper formate tetrahydrate is added to the mixed solution, stirred in a closed container until completely dissolved, and filtered through a microporous filter membrane to obtain a particle-free copper conductive ink.
4. The method for preparing a particle-free copper conductive ink for 3D inkjet printing according to claim 3, characterized in that: In step (1), the mixing time is 0.5 h to 5 h; in step (2), the stirring time is 5 to 10 h; and filtering is performed sequentially using microporous filter membranes with pore sizes of 450 nm and 220 nm.
5. A conductive copper film, characterized in that: The particle-free copper conductive ink as claimed in claim 1 or 2 is prepared by 3D inkjet printing.
6. A method for preparing a conductive copper film according to claim 5, characterized in that: The method comprises the following steps: printing particle-free copper conductive ink on a flexible substrate by a microelectronic inkjet printer 3D, and sintering the ink in an inert gas or reducing gas atmosphere to obtain a conductive copper film.
7. The method for preparing a conductive copper film according to claim 6, characterized in that: The sintering temperature is 150°C-300°C, and the sintering time is 1min-15min.
8. The method for preparing a conductive copper film according to claim 6, characterized in that: The flexible substrate is cyanate, polyethylene terephthalate or a quartz sheet.
Citation Information
Cited By
Copper conductive ink material preparation device and method
CN119869293A