Ceramicizable lightweight organic silicon anti-heat insulation coating and preparation method thereof

By adding ceramic additives and ceramic fillers to the silicone coating, combining hollow ceramic microspheres and basalt fibers to form a ceramic body, the problems of difficulty in curing and poor heat resistance of existing coatings at high temperatures are solved, and the problem of existing coatings is achieved. Highly efficient and low-cost pneumatic thermal protection effect.

CN116285673BActive Publication Date: 2024-11-22HUBEI SANJIANG AEROSPACE JIANGHE CHEM TECH

Patent Information

Application Number
CN202211568391.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-11-22
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The existing silicone thermal protection coatings have problems such as difficulty in deep curing, poor thermal resistance and ablation resistance, cumbersome construction and high cost during high temperature and long-term use, and cannot meet the problems of long-term and high-thermal flow density aerodynamic heat of hypersonic vehicles. environmental requirements.

Method used

Coating A with a mass ratio of 100: 0.3-5.0 is mixed with coating B. Coating A includes double-end vinyl silicone oil, end-side vinyl silicone oil, curing agent, reinforcement filler, lightweight heat insulation filler, high-temperature resistant filler , ceramicizing additives, ceramicized fillers, ablation-resistant fibers and diluents, and ceramicized lightweight silicone heat-proof insulation coating is obtained through spraying and curing, and high-temperature ceramicization reaction is carried out using ceramicizing additives and ceramicized fillers. , combined with hollow ceramic microspheres and basalt fiber support, form a hard ceramic body.

Benefits of technology

The coating is achieved with low density, high mechanical properties, controllable curing rate and deep curing, which significantly improves the coating's anti-ablation and anti-shrink performance, reduces construction complexity and cost, and meets high-temperature and efficient pneumatic heat Protection needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285673B_ABST
    Figure CN116285673B_ABST
Patent Text Reader

Abstract

The present invention provides a ceramicized lightweight organic silicon anti-insulation coating and a preparation method thereof, wherein the coating is obtained by mixing coating A and coating B in a mass ratio of 100:0.3-5.0, and coating and curing; wherein coating A includes double-end-capped vinyl silicone oil, end-side vinyl silicone oil, curing agent, reinforcing filler, lightweight insulation filler, high temperature resistant filler, ceramicizing aid, ceramicizing filler, ablation-resistant fiber, curing inhibitor and diluent; coating B component is a curing catalyst with a concentration of 500-5000ppm. The coating adopts addition-type silicone oil as a curing system, which can be thoroughly cured without releasing small molecules, has a low curing shrinkage rate, and the coating thickness quality is easy to control. Under high-temperature ablation, the coating surface is ceramicized to form a hard ceramic body to prevent further ablation of the coating, so that the coating has good ablation resistance, erosion resistance and thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lightweight, high-temperature-resistant and anti-scour coating protection, and specifically relates to a ceramic lightweight organic silicon anti-heat-insulating coating and a preparation method thereof. Background Art

[0002] Due to the aerodynamic thermal effect, the surface temperature of an aircraft can reach thousands of degrees during flight. In order to prevent the temperature from being too high during the operation of the aircraft, which may cause the shell to lose strength and cause structural damage, thermal protection measures need to be taken on the outside of the aircraft shell to reduce the impact of aerodynamic heat on the aircraft shell and control system, and ensure the success of the flight mission. With the continuous development of hypersonic aircraft technology, the flight speed of modern aircraft can reach 5-10 Mach, which puts higher requirements on the performance of thermal insulation materials. Organic silicon coatings have become the mainstream of current aircraft resin-based thermal protection materials due to their advantages such as room temperature curing, outstanding high temperature resistance, good low temperature resistance, high elongation, and convenient construction. At present, the common organic silicon thermal protection coatings on the market use condensation-type phenyl silicone rubber, which mainly uses hydroxyl-terminated methyl phenyl silicone rubber as the base rubber, orthosilicate compounds and organic tin reagents as the curing system, supplemented by reinforcing fillers, lightweight fillers, heat-resistant fillers and other functional additives. However, this type of coating has the disadvantages of difficult deep curing and poor heat resistance and ablation resistance. As the working time increases, the coating gradually peels off, causing it to lose its thermal protection performance and cannot be used in long-term, high heat flux density aerodynamic thermal environments. CN109161331A discloses a ceramic spiral fiber reinforced silicone rubber lightweight ablation-resistant thermal insulation coating and its application. Its disadvantage is that the preparation process of the raw material ceramic spiral fiber is relatively complicated, and the use of condensation-type silicone rubber as the base glue will result in a high coating curing shrinkage rate, resulting in difficulty in controlling the thickness of the two layers of coating, cumbersome construction, and a long construction process. CN109796870A discloses a ceramic ablation-resistant silicone rubber composite material coating and a preparation method for its coating. Its disadvantage is that its base glue is phenyl silicone rubber, which is expensive. Based on this, the development of a low-cost, high-temperature ceramic coating formula with readily available raw materials to prevent it from peeling off under aerodynamic heat and meet the needs of long-flight, high heat flux density aerodynamic thermal protection aircraft is of great significance to the development of my country's aerospace industry and national defense technology. Summary of the invention

[0003] The present invention provides a ceramicized lightweight organic silicon anti-heat insulation coating and a preparation method thereof, which has the advantages of cheap and readily available raw materials, simple and convenient construction, low density, excellent mechanical properties, good process performance, controllable curing rate and deep curing, small curing shrinkage, good ablation resistance, especially good oxygen-enriched ablation performance.

[0004] The technical solution of the present invention is a ceramicized lightweight organic silicon anti-heat insulation coating, which is obtained by mixing coating A and coating B in a mass ratio of 100:0.3-5.0, and then coating and curing;

[0005] The coating A comprises the following raw materials in parts by mass: 70-100 parts of double-terminated vinyl silicone oil, 10-30 parts of end-side vinyl silicone oil, 2-10 parts of curing agent, 10-30 parts of reinforcing filler, 50-90 parts of lightweight heat-insulating filler, 0.5-4 parts of high-temperature resistant filler, 5-20 parts of ceramic additive, 10-30 parts of ceramic filler, 5-20 parts of ablation-resistant fiber, 0.5-3 parts of curing inhibitor, and 30-70 parts of diluent;

[0006] The coating component B is a curing catalyst with a concentration of 500-5000 ppm.

[0007] Furthermore, the double-terminated vinyl silicone oil is methyl vinyl silicone oil or methylphenyl vinyl silicone oil, with a vinyl content of 0.06%-0.32%. The preferred end-side vinyl silicone oil is methyl vinyl silicone oil, with a vinyl content of 2.30%-6.00%.

[0008] Furthermore, the terminal vinyl silicone oil is methyl vinyl silicone oil or methylphenyl vinyl silicone oil, with a vinyl content of 1.50%-8.00%; preferably, the terminal vinyl silicone oil is methyl vinyl silicone oil, with a vinyl content of 2.30%-6.00%.

[0009] Furthermore, the curing agent is hydrogen-containing silicone oil, and the hydrogen content is 0.23%-1.30%, preferably 0.50%-0.90%.

[0010] Furthermore, the reinforcing filler is fumed silica, nano-scale carbon black or a mixture of the two; the lightweight heat-insulating filler is one of hollow ceramic microspheres, hollow glass microspheres, and hollow phenolic microspheres; preferably hollow ceramic microspheres. Compared with hollow glass microspheres, hollow ceramic microspheres have the characteristics of low density, low thermal conductivity, and high softening point. At high temperatures, they are less likely to soften, which can effectively ensure that the ceramic body does not deform excessively. The high-temperature resistant filler is one or a combination of iron oxide, cerium oxide, and zirconium oxide. Iron oxide is preferred, which can effectively absorb the free radicals released by the decomposition of silicone rubber, thereby improving the heat resistance of silicone rubber.

[0011] Furthermore, the ceramicizing aid is one or a combination of low-melting-point glass powder, low-melting-point ceramic powder, and zinc borate; preferably, low-melting-point glass powder.

[0012] The ceramic filler is one or a combination of muscovite, kaolin, wollastonite, diatomaceous earth, and montmorillonite; preferably wollastonite. The ablation-resistant fiber is one or a combination of glass fiber, high silica fiber, basalt fiber, and mullite fiber. Basalt fiber is preferred. Compared with other fibers, basalt fiber has the characteristics of low price and good compatibility with silicone rubber. Through the ceramicizing additive, the ceramic filler undergoes a ceramicizing reaction at high temperature, and at the same time, the basalt fiber and the hollow ceramic microspheres support the skeleton, so that the generated ceramic body has a higher strength and will not be excessively deformed.

[0013] Furthermore, the curing inhibitor is one of 2-methyl-3-butyn-2-ol, 1-ethynylcyclohexanol, diallyl maleate, and diethyl fumarate, preferably 2-methyl-3-butyn-2-ol and 1-ethynylcyclohexanol.

[0014] Further, the diluent is one or a combination of 120 solvent oil, butyl acetate, xylene or toluene, preferably 120 solvent oil and / or butyl acetate.

[0015] Furthermore, the curing catalyst is a Custer catalyst with a concentration of 500-5000 ppm.

[0016] The present invention also relates to a method for preparing the coating, the specific steps of which are:

[0017] S1. Mix the double-terminated vinyl silicone oil, the end-side vinyl silicone oil, the curing agent, the curing inhibitor and the reinforcing filler in proportion; then add the high temperature resistant filler, the ceramic additive, the ceramic filler and the ablation resistant fiber and mix them; finally, add the light heat insulating filler and the diluent and mix them to obtain component A;

[0018] S2: When preparing the coating, add a diluent to component A to dilute it to the spraying viscosity, add component B and mix evenly, then spray it. The thickness of each spraying is 0.2-0.4mm, and the interval between each spraying is 15-30min. Repeat the spraying until the required thickness is reached and solidify.

[0019] Furthermore, after spraying, the coating is cured at room temperature for 1-3 days or placed at room temperature for 12 hours and then cured at 70°C for 1-3 hours to obtain the target ceramicized lightweight silicone anti-heat-insulating coating.

[0020] The present invention has the following beneficial effects:

[0021] 1. The base glue system of the present invention is a mixture of double-terminated vinyl silicone oil and end-side vinyl silicone oil, which adjusts the cross-linking network and concentrated cross-linking points of the coating curing system, further adjusts the curing ratio by the curing agent, and adjusts the reinforcing system by the reinforcing filler, thereby adjusting the tensile strength and elongation at break of the coating material, the construction cycle can be adjusted, and the curing temperature and speed can be controlled. The mechanical properties of the coating can be greatly improved, so that the coating has excellent tensile strength.

[0022] 2. The present invention adopts addition-type silicone rubber as the resin curing system, which has the advantages of low cost, excellent mechanical properties of the prepared coating, low curing volume shrinkage, and deep vulcanization, thereby ensuring that the material thickness quality is controllable.

[0023] 3. The present invention adopts addition-type organic silicone rubber as the resin curing system, which avoids the residual hydroxyl group after the condensation-type silicone rubber is cured, resulting in a decrease in the heat resistance of the coating, and improves the ablation and erosion resistance of the coating.

[0024] 4. The present invention uses high temperature resistant hollow ceramic microspheres as lightweight thermal insulation fillers, which have the characteristics of high softening point and can effectively inhibit high temperature deformation of the coating, and have good high temperature maintenance capabilities.

[0025] 5. The ceramic flame retardant system used in the present invention can effectively enhance the ablation and scour resistance of the silicone rubber coating. At high temperatures, a hard ceramic body is formed on the surface of the coating, which can effectively resist aerodynamic thermal scour (especially aerodynamic scour in an oxygen-rich environment) and prevent further ablation of the silicone rubber, thereby improving the ablation and scour resistance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A 2.5 mm thick coating prepared from the material obtained in Examples 1-5 was placed at 800° C. for 5 minutes and then illuminated from the front.

[0027] Figure 2 A 2.5 mm thick coating prepared from the material obtained in Examples 1-5 was placed at 800° C. for 5 minutes and back-illuminated. DETAILED DESCRIPTION

[0028] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0029] Example 1

[0030] (1) Add 100 g of double-end-capped methyl vinyl silicone oil (vinyl content 0.10%), 10 g of end-side methyl vinyl silicone oil (vinyl content 2.31%), 3.0 g of hydrogen-containing silicone oil (hydrogen content 0.52%), 0.5 g of 2-methyl-3-butyn-2-ol, 20 g of fumed silica, and 1.0 g of nano carbon black into a barrel, use a wooden spatula to mix the components evenly until there are no obvious agglomerates, and grind them on a three-roll grinder for 4 times to obtain a grind.

[0031] (2) Add 2.0 g of iron oxide, 15 g of low-melting-point glass powder, 15 g of muscovite, and 15 g of glass fiber to the ground material, use a wooden shovel to mix the components evenly until there is no obvious agglomeration of particles, and grind on a three-roll mill for 4 times to obtain a mixture.

[0032] (3) Add 70 g of hollow glass microspheres and 40 g of butyl acetate to the mixture, and mix them for 30 min using a pneumatic stirrer at a mixing rate of 150 r / min to obtain coating component A. Component B uses a commercially available Custer catalyst.

[0033] (4) Use 120 solvent oil to dilute the viscosity of component A of the coating to 20-30 seconds for coating four cups. Add component B according to the ratio of component A: component B = 100:1.5, further mix evenly, and then use an air spray gun to spray on the surface of the sample. The air pressure during spraying is (0.4-0.6) MPa, the diameter of the spray gun is 3.0 mm, the distance between the spray gun and the sample is 150-300 mm, the thickness of each spray is 0.2-0.4 mm, and the interval between each spray is 20 minutes. Repeat the spraying until the specified thickness is reached.

[0034] (5) The sprayed sample is placed in an environment with room temperature and a water content of less than 75% for curing for 3 days, or placed in an environment with room temperature for 24 hours and then cured in an environment with a water content of less than 75% for 3 hours, and the relevant performance tests are performed on the sample.

[0035] Example 2

[0036] (1) Add 80 g of double-end-capped methyl vinyl silicone oil (vinyl content 0.13%), 20 g of end-side methyl vinyl silicone oil (vinyl content 3.69%), 4.5 g of hydrogen-containing silicone oil (hydrogen content 0.79%), 0.8 g of 1-ethynylcyclohexanol, 25 g of fumed silica, and 1.5 g of nano carbon black into a barrel, use a wooden spatula to mix the components evenly until there are no obvious agglomerates, and grind them on a three-roll grinder for 4 times to obtain a grind.

[0037] (2) Add 1.0 g of iron oxide, 17 g of low-melting-point glass powder, 20 g of diatomaceous earth, and 18 g of basalt fiber to the ground material, use a wooden shovel to mix the components evenly until there is no obvious agglomeration of particles, and grind on a three-roll mill for 4 times to obtain a mixture.

[0038] (3) Add 70 g of hollow ceramic microspheres and 40 g of butyl acetate to the mixture, and mix them for 30 min using a pneumatic stirrer at a mixing rate of 150 r / min to obtain coating component A. Component B uses a commercially available Custer catalyst.

[0039] (4) Use 120 solvent oil to dilute the viscosity of component A of the coating to 20-30 seconds for coating four cups. Add component B according to the ratio of component A: component B = 100:2.3, further mix evenly, and then use an air spray gun to spray on the surface of the sample. The air pressure during spraying is (0.4-0.6) MPa, the diameter of the spray gun is 3.0 mm, the distance between the spray gun and the sample is 150-300 mm, the thickness of each spray is 0.2-0.4 mm, and the interval between each spray is 20 minutes. Repeat the spraying until the specified thickness is reached.

[0040] (5) The sprayed sample is placed in an environment with room temperature and a water content of less than 75% for curing for 3 days, or placed in an environment with room temperature for 24 hours and then cured in an environment with a water content of less than 75% for 3 hours, and the relevant performance tests are performed on the sample.

[0041] Example 3

[0042] (1) Add 90 g of double-terminated methyl vinyl silicone oil (vinyl content 0.16%), 30 g of end-side methyl vinyl silicone oil (vinyl content 8.10%), 6.0 g of hydrogen-containing silicone oil (hydrogen content 0.98%), 1.0 g of 1-ethynyl cyclohexanol, 18 g of fumed silica, and 2 g of nano carbon black into a barrel, mix the components evenly with a wooden shovel until there are no obvious agglomerates, and grind them on a three-roll grinder for 4 times to obtain a grinding material.

[0043] (2) Add 1.0 g of iron oxide, 10 g of low melting point ceramic powder, 25 g of wollastonite, and 10 g of basalt fiber to the grinding material, use a wooden shovel to mix the components evenly until there is no obvious particle agglomeration, and grind them on a three-roll mill for 4 times to obtain a mixed material.

[0044] (3) Add 80 g of hollow ceramic microspheres and 50 g of toluene to the mixture, and mix them for 30 min using a pneumatic stirrer at a mixing rate of 150 r / min to obtain coating component A. Component B uses a commercially available Custer catalyst.

[0045] (4) Use 120 solvent oil to dilute the viscosity of component A of the coating to 20-30 seconds for coating four cups. Add component B according to the ratio of component A: component B = 100:3.5, further mix evenly, and then use an air spray gun to spray on the surface of the sample. The air pressure during spraying is (0.4-0.6) MPa, the diameter of the spray gun is 3.0 mm, the distance between the spray gun and the sample is 150-300 mm, the thickness of each spray is 0.2-0.4 mm, and the interval between each spray is 20 minutes. Repeat the spraying until the specified thickness is reached.

[0046] (5) Place the sprayed sample at room temperature and a water content of less than 75% for 3 days, or place it at room temperature for 24 hours and then cure it at 70°C and a water content of less than 75% for 3 hours, and then conduct relevant performance tests on the sample.

[0047] Example 4

[0048] (1) Add 80 g of double-terminated methyl vinyl silicone oil (vinyl content 0.13%), 20 g of end-side methyl vinyl silicone oil (vinyl content 2.31%), 4.9 g of hydrogenated silicone oil (vinyl content 0.79%), 1.2 g of 2-methyl-3-butyn-2-ol, 28 g of fumed silica, and 1.5 g of nano carbon black into a barrel, mix the components evenly with a wooden shovel until there are no obvious agglomerates, and grind them on a three-roll grinder for 4 times to obtain a grinding material.

[0049] (2) Add 0.5 g of iron oxide, 18 g of low-melting-point glass powder, 23 g of kaolin, and 16 g of high-silica fiber to the grinding material, use a wooden shovel to mix the components evenly until there is no obvious particle agglomeration, and grind them on a three-roll mill for 4 times to obtain a mixed material.

[0050] (3) Add 60 g of hollow ceramic microspheres and 38 g of butyl acetate to the mixture, and mix them for 30 min using a pneumatic stirrer at a mixing rate of 150 r / min to obtain coating component A. Component B uses a commercially available Custer catalyst.

[0051] (4) Use 120 solvent oil to dilute the viscosity of component A of the coating to 20-30 seconds for coating four cups. Add component B according to the ratio of component A: component B = 100:4.5, further mix evenly, and then use an air spray gun to spray on the surface of the sample. The air pressure during spraying is (0.4-0.6) MPa, the diameter of the spray gun is 2.0 mm, the distance between the spray gun and the sample is 150-300 mm, the thickness of each spray is 0.2-0.4 mm, and the interval between each spray is 15 minutes. Repeat the spraying until the specified thickness is reached.

[0052] (5) Place the sprayed sample in an environment with room temperature and water content less than 75% for curing for 3 days, or place it in an environment with room temperature for 24 hours and then cure it in an environment with water content less than 75% for 3 hours at 70℃, and then conduct relevant performance tests on the sample.

[0053] Example 5

[0054] (1) Add 85 g of double-terminated methyl vinyl silicone oil (vinyl content 0.13%), 15 g of end-side methyl vinyl silicone oil (vinyl content 3.69%), 4.0 g of hydrogen-containing silicone oil (hydrogen content 0.79%), 0.9 g of tetramethyltetravinylcyclotetrasiloxane, 22 g of fumed silica, and 0.8 g of nano carbon black into a barrel, mix the components evenly with a wooden shovel until there is no obvious agglomeration, and grind on a three-roll mill for 4 times to obtain a grinding material.

[0055] (2) Add 1.3 g of zirconium oxide, 12 g of low-melting-point glass powder, 16 g of montmorillonite, and 10 g of high-silica fiber to the ground material, use a wooden shovel to mix the components evenly until there is no obvious particle agglomeration, and grind them on a three-roll mill for 4 times to obtain a mixed material.

[0056] (3) Add 60 g of hollow glass microspheres and 50 g of 120 solvent oil to the mixture, and mix them for 30 min using a pneumatic stirrer at a mixing rate of 150 r / min to obtain coating component A. Component B uses a commercially available Custer catalyst.

[0057] (4) Use 120 solvent oil to dilute the viscosity of component A of the coating to 20-30 seconds for coating four cups. Add component B according to the ratio of component A: component B = 100:3.0, further mix evenly, and spray it on the surface of the sample with an air spray gun. The air pressure during spraying is (0.4-0.6) MPa, the diameter of the spray gun is 2 mm, the distance between the spray gun and the sample is 150-300 mm, the thickness of each spray is 0.2-0.4 mm, and the interval between each spray is 15 minutes. Repeat the spraying until the specified thickness is reached.

[0058] (5) The sprayed sample is placed in an environment with room temperature and a water content of less than 75% for curing for 3 days, or placed in an environment with room temperature for 24 hours and then cured in an environment with a water content of less than 75% for 3 hours, and the relevant performance tests are performed on the sample.

[0059] Comparative Example 1: Based on Example 2, the difference is that it contains only 100g of di-terminated methyl vinyl silicone oil (vinyl content 0.13%) and does not contain terminal methyl vinyl silicone oil.

[0060] Comparative Example 2: Based on Example 2, the difference is that no curing inhibitor is added. Under this condition, the coating cures too fast and cannot meet the requirements of the spraying process.

[0061] Comparative Example 3: Based on Example 2, the difference is that it contains only 100g of terminal methyl vinyl silicone oil (vinyl content 3.69%) and does not contain di-terminated methyl vinyl silicone oil. The coating prepared is a brittle coating without elasticity.

[0062] The properties of the coatings obtained in Examples 1 to 5 and Comparative Example 1 are specifically shown in Table 1 below.

[0063] Table 1 Measured performance of the embodiment

[0064]

[0065] In addition, the 2.5 mm thick coating prepared from the materials obtained in Examples 1-5 was placed at 800°C for 5 minutes and the front and back surfaces were illuminated. Figure 1 and Figure 2 As can be seen from the figure, the coating undergoes a ceramic reaction at 800°C to form a hard ceramic body, and the coating does not deform, bubble, or crack. This shows that the coating has good heat-resistant aerodynamic shape-maintaining ability.

[0066] The above embodiments describe the preferred implementation of the present invention, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A ceramicized lightweight organic silicon anti-heat insulation coating, characterized in that: The coating is obtained by mixing coating A and coating B in a mass ratio of 100:0.3-5.0, and then coating and curing. Wherein, coating A comprises the following raw materials in parts by mass: 70-100 parts of double-terminated vinyl silicone oil, 10-30 parts of end-side vinyl silicone oil, 2-10 parts of hydrogen-containing silicone oil with a hydrogen content of 0.23%-1.30% as a curing agent, 10-30 parts of reinforcing filler, 50-90 parts of hollow ceramic microspheres as a lightweight heat-insulating filler, 0.5-4 parts of iron oxide as a high-temperature resistant filler, 5-20 parts of low-melting-point glass powder as a ceramicizing aid, 10-30 parts of wollastonite as a ceramicizing filler, 5-20 parts of basalt fiber as an ablation-resistant fiber, 0.5-3 parts of a curing inhibitor, and 30-70 parts of a diluent; the double-terminated vinyl silicone oil is methyl vinyl silicone oil or methylphenyl vinyl silicone oil, with a vinyl content of 0.06%-0.32%; the end-side vinyl silicone oil is methyl vinyl silicone oil or methylphenyl vinyl silicone oil, with a vinyl content of 1.50%-8.00%; The coating component B is a curing catalyst with a concentration of 500-5000ppm; The specific steps for coating preparation are: S1. Mix the double-terminated vinyl silicone oil, the end-side vinyl silicone oil, the curing agent, the curing inhibitor and the reinforcing filler in proportion; then add the high temperature resistant filler, the ceramic additive, the ceramic filler and the ablation resistant fiber and mix them; finally, add the light heat insulating filler and the diluent and mix them to obtain component A; S2: When preparing the coating, add a diluent to component A to dilute it to the spraying viscosity, add component B and mix evenly, then spray it. The thickness of each spraying is 0.2-0.4mm, and the interval between each spraying is 15-30min. Repeat the spraying until the required thickness is reached and solidify.

2. The coating according to claim 1, characterized in that: The reinforcing filler is fumed silica, nano-scale carbon black or a mixture of the two.

3. The coating according to claim 1, characterized in that: The curing inhibitor is one of 2-methyl-3-butyn-2-ol, 1-ethynylcyclohexanol, diallyl maleate, and diethyl fumarate.

4. The coating according to claim 1, characterized in that: The diluent is one or a combination of 120 solvent oil, butyl acetate, xylene or toluene.

5. The coating according to claim 1, characterized in that: The curing catalyst is a Custer catalyst with a concentration of 500-5000ppm.

6. The coating according to claim 1, characterized in that: After spraying, the coating is cured at room temperature for 1-3 days or placed at room temperature for 12 hours and then cured at 70°C for 1-3 hours to obtain the target ceramicized lightweight organic silicon anti-heat insulation coating.

Citation Information

Patent Citations

  • Ceramic spiral fiber reinforced silicone rubber light ablation resistance thermal insulation coating and application thereof

    CN109161331A

  • Ceramic ablation-resistant silicone rubber composite material paint and preparation method of coating thereof

    CN109796870A

  • Ablation-resisting light silicone rubber thermal insulation coating

    CN110054992A

  • Self-repairing ceramic silicone rubber material and preparation method thereof

    CN110183858A

  • Preparation and process of in-situ ceramic high-temperature resistance heat insulation coating

    CN110479564A

Cited By

  • Gradient functional coating containing hollow glass beads as well as preparation method and application of gradient functional coating

    CN122278342A