A coating with high heat sealing strength and high barrier performance and a preparation method thereof
By adding cross-linked collagen fibers, starch, nanocellulose and sodium alginate to cellulose paper to form a paint with a dual network structure, the problem of insufficient barrier and mechanical properties of cellulose paper in the food packaging field is solved, and the problem of insufficient barrier and mechanical properties of cellulose paper in the field of food packaging is achieved. It has improved the high heat seal strength and barrier properties, and the paint is non-toxic, environmentally friendly and degradable, expanding its application range.
Patent Information
- Application Number
- CN202310366091.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Existing cellulose papers are difficult to meet the needs of high barrier and high mechanical properties in the food packaging field, and the use of plastic coatings leads to difficulties in degrading and recycling of materials.
By crosslinking collagen fibers with glutaraldehyde and added gelatinized starch, nanocellulose and sodium alginate, a dual network structure is formed to enhance the film-forming performance of the coating and cross-link with calcium chloride to form a high heat sealing strength. High barrier properties coating.
The coating gives paper strong mechanical properties, high barrier properties and high heat seal strength, expands the application range in the food packaging field, and is non-toxic, environmentally friendly and degradable.
Smart Images

Figure BDA0004166733480000071 
Figure BDA0004166733480000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional materials, and in particular relates to a coating with high heat sealing strength and high barrier performance and a preparation method thereof. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] Cellulose is a widely available, biocompatible, and environmentally biodegradable natural biopolymer for paper-based materials. For food packaging, paper materials must possess excellent mechanical, barrier, and heat-sealing properties to meet market demand. However, cellulose-based paper alone falls far short of achieving ideal physical performance targets. To meet product requirements (oil resistance, water resistance, barrier properties, and sealing), some manufacturers employ simple plastic coatings to impart superior properties. However, the presence of these coatings makes degradation and recycling of paper products extremely difficult.
[0004] Heat-sealed bags are widely used in food packaging. As a food material, film packaging materials must possess excellent impact resistance and sealing strength during storage and transportation to prevent external conditions from releasing food from the bag. Furthermore, improving the barrier properties of food packaging bags can effectively block external contaminants and prevent rapid food spoilage. Collagen fibers are edible and have good film-forming properties, but their mechanical and barrier properties are poor, making them difficult to meet the high barrier and mechanical performance requirements of food packaging materials. Summary of the Invention
[0005] In response to the shortcomings of the existing technology, the purpose of the present invention is to provide a high heat seal strength and high barrier performance coating and a preparation method thereof. The coating film formed by coating the coating gives paper strong mechanical properties, high barrier properties and high heat seal strength, expanding the application range in the field of food packaging.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a coating with high heat seal strength and high barrier performance, comprising the following steps:
[0008] After the collagen fibers are heated and dissolved, glutaraldehyde is added thereto for cross-linking. The amount of glutaraldehyde added is 1%-10% of the mass of the collagen fibers. The mixture is stirred and reacted for 0.5-1h.
[0009] After the reaction is completed, gelatinized starch, nanocellulose and sodium alginate are added in sequence and stirred under heating conditions; the amount of starch added is 20%-50% of the mass of the collagen fiber, the amount of nanocellulose added is 10%-20% of the mass of the collagen fiber; the amount of sodium alginate added is 3%-10% of the mass of the collagen fiber; the amount of calcium chloride added is 1%-5% of the mass of the sodium alginate, and the reaction is stirred for 1-1.5 hours to obtain the coating.
[0010] The addition of gelatinized starch and nanocellulose improves the barrier and mechanical properties of the film through intermolecular physical interactions; the sodium alginate and calcium chloride are cross-linked again to form a double network structure to enhance the mechanical and barrier properties of the film.
[0011] Nanomaterials have high specific surface areas and more binding sites. Among them, nanocellulose is green, biodegradable, has good water retention, a large specific surface area, and good physical properties and thermal stability.
[0012] In some embodiments, the temperature for heating and dissolving the collagen fibers is 40-65°C.
[0013] In some embodiments, when starch, nanocellulose and sodium alginate are added to the collagen fibers in sequence, each substance is mixed evenly before adding the next substance.
[0014] In some embodiments, the amount of glutaraldehyde added is 5%-8% of the mass of the collagen fibers.
[0015] In some embodiments, the amount of starch added is 30%-40% of the mass of the collagen fibers.
[0016] Preferably, during the starch addition process, the temperature of the collagen fibers is 35-45°C. , Avoid thermal decomposition of collagen fibers at high temperatures.
[0017] Preferably, the starch is selected from one or a combination of corn starch, pea starch, native starch or cationic tapioca starch.
[0018] In some embodiments, the amount of nanocellulose added is 15%-18% of the collagen fibers, the stirring temperature is 35-45° C., and the stirring time is 20-30 min.
[0019] In some embodiments, the method further includes the steps of uniformly coating the prepared coating on paper and drying the paper to prepare the wrapping paper.
[0020] Preferably, the specification of the coating rod is 5-50 μm, and the coating amount is 1-10 g / m 2 .
[0021] More preferably, the specification of the coating rod is 5-20 μm, and the coating amount is 2-5 g / m 2 .
[0022] In a second aspect, the present invention provides a coating with high heat-sealing strength and high barrier performance, which is prepared by the above-mentioned preparation method.
[0023] In a third aspect, the present invention provides a food packaging paper, wherein a packaging film is coated on a paper base, and the packaging film is prepared by coating with the coating and then drying.
[0024] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0025] The coating film formed by applying the coating gives paper strong mechanical properties, high barrier properties and high heat sealing strength, expanding its application range in the field of food packaging.
[0026] The coating liquid is non-toxic, environmentally friendly, and biodegradable. It can be applied to a variety of papers and is widely used in food, medicine and other fields. DETAILED DESCRIPTION
[0027] It should be noted that the following detailed description is illustrative and is intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meaning as commonly understood by those skilled in the art to which the present invention belongs.
[0028] The present invention will be further described below with reference to the embodiments.
[0029] Example 1
[0030] (1) 30 g of collagen fibers were dissolved by stirring at 45°C, and then 6% glutaraldehyde was added and stirred for 0.5 h to allow for full reaction.
[0031] (2) adding 35% starch (relative to the collagen fiber) to the collagen fiber solution after the reaction in step (1), stirring at 45° C. for 1 h to mix uniformly;
[0032] (3) adding 15% nanocellulose (relative to collagen fibers) to the mixed solution in step (2) and stirring at 45° C. for 20 minutes to mix uniformly;
[0033] (4) Add 6% sodium alginate (relative to collagen fibers) to the mixed solution obtained in step (3), stir at 45°C for 0.5 h to mix evenly, then add 3% calcium chloride (relative to sodium alginate), and continue stirring for 1 h to allow for uniform reaction;
[0034] (5) The heat-sealable, high-barrier coating solution obtained in step (4) is evenly coated on the tissue paper using a coating machine and dried at room temperature (the coating rod size is 10 μm).
[0035] Example 2
[0036] (1) 30 g of collagen fibers were dissolved by stirring at 45°C, and then 6% glutaraldehyde was added and stirred for 0.5 h to allow for full reaction.
[0037] (2) adding 20% (Example 2-1) or 50% starch (relative to the collagen fibers) (Example 2-2) to the collagen fiber solution after the reaction in step (1), stirring at 45° C. for 1 h to mix uniformly;
[0038] (3) adding 15% nanocellulose (relative to collagen fibers) to the mixed solution in step (2) and stirring at 45° C. for 20 minutes to mix uniformly;
[0039] (4) Add 6% sodium alginate (relative to collagen fibers) to the mixed solution obtained in step (3), stir at 45°C for 0.5 h to mix evenly, then add 3% calcium chloride (relative to sodium alginate), and continue stirring for 1 h to allow for uniform reaction;
[0040] (5) The heat-sealable, high-barrier coating solution obtained in step (4) is evenly coated on the tissue paper using a coating machine and dried at room temperature (the coating rod size is 10 μm).
[0041] Example 3
[0042] (1) 30 g of collagen fibers were dissolved by stirring at 45°C, and then 6% glutaraldehyde was added and stirred for 0.5 h to allow for full reaction.
[0043] (2) adding 35% starch (relative to the collagen fiber) to the collagen fiber solution after the reaction in step (1), stirring at 45° C. for 1 h to mix uniformly;
[0044] (3) Add 10% (Example 3-1) or 20% (Example 3-2) of nanocellulose (relative to collagen fibers) to the mixed solution in step (2), and stir at 45°C for 20 minutes to mix evenly;
[0045] (4) Add 6% sodium alginate (relative to collagen fibers) to the mixed solution obtained in step (3), stir at 45°C for 0.5 h to mix evenly, then add 3% calcium chloride (relative to sodium alginate), and continue stirring for 1 h to allow for uniform reaction;
[0046] (5) The heat-sealable, high-barrier coating solution obtained in step (4) is evenly coated on the tissue paper using a coating machine and dried at room temperature (the coating rod size is 10 μm).
[0047] Example 4
[0048] (1) 30 g of collagen fibers were dissolved by stirring at 45°C, and then 6% glutaraldehyde was added and stirred for 0.5 h to allow for full reaction.
[0049] (2) adding 35% starch (relative to the collagen fiber) to the collagen fiber solution after the reaction in step (1), stirring at 45° C. for 1 h to mix uniformly;
[0050] (3) adding 15% nanocellulose (relative to collagen fibers) to the mixed solution in step (2) and stirring at 45° C. for 20 minutes to mix uniformly;
[0051] (4) 6% sodium alginate (relative to collagen fibers) was added to the mixed solution obtained in step (3), and the mixture was stirred at 45°C for 0.5 h to mix uniformly. Then, 1% (Example 4-1) or 5% calcium chloride (relative to sodium alginate) (Example 4-2) was added, and the mixture was stirred for 1 h to allow for uniform reaction.
[0052] (5) The heat-sealable, high-barrier coating solution obtained in step (4) is evenly coated on the tissue paper using a coating machine and dried at room temperature (the coating rod size is 10 μm).
[0053] Example 5
[0054] (1) 30 g of collagen fibers were dissolved by stirring at 45°C, and then 6% glutaraldehyde was added and stirred for 0.5 h to allow for full reaction.
[0055] (2) adding 35% starch (relative to the collagen fiber) to the collagen fiber solution after the reaction in step (1), stirring at 45° C. for 1 h to mix uniformly;
[0056] (3) adding 15% nanocellulose (relative to collagen fibers) to the mixed solution in step (2) and stirring at 45° C. for 20 minutes to mix uniformly;
[0057] (4) Add 5% (Example 5-1) and 8% sodium alginate (relative to collagen fibers) (Example 5-2) to the mixed solution obtained in step (3), stir at 45°C for 0.5 h to mix evenly, then add 3% calcium chloride (relative to sodium alginate), and continue stirring for 1 h to allow for uniform reaction;
[0058] (5) The heat-sealable, high-barrier coating solution obtained in step (4) is evenly coated on the tissue paper using a coating machine and dried at room temperature (the coating rod size is 10 μm).
[0059] Comparative Example 1
[0060] Step (2) in Example 1 was omitted, and other conditions were consistent with those in Example 1.
[0061] Comparative Example 2
[0062] Step (3) in Example 1 was omitted, and other conditions were consistent with those in Example 1.
[0063] Comparative Example 3
[0064] Step (2) and step (3) in Example 1 were omitted, and other conditions were consistent with those in Example 1.
[0065] Comparative Example 4
[0066] Step (4) in Example 1 was omitted, and other conditions were consistent with those in Example 1.
[0067] The performance data of the collagen fiber-based composite films prepared in various examples and comparative examples are listed in Table 1.
[0068] Table 1 Performance data of composite films prepared in various embodiments and comparative examples
[0069]
[0070]
[0071] Summary and Conclusion
[0072] As can be seen from the above examples, the preparation method of the present invention is simple and only uses physical mixing to make a coating liquid, which is then applied to the surface of tissue paper (or other types of paper) by coating. By comprehensively adjusting the ratio of the raw materials, paper with high mechanical properties, barrier properties, and heat-sealing properties can be obtained. In particular, when the starch addition amount is 35%, the nanocellulose addition amount is 15%, the sodium alginate addition amount is 6%, and the calcium chloride addition amount is 3%, and the coating is performed using a 10μm scraper, the tensile strength is 35MPa, the heat-sealing strength reaches 30N / 15mm, and the water vapor transmission rate is as low as 1.889×10 -13 g·m -1 ·s -1 ·Pa -1 .
[0073] In addition, the coating liquid is non-toxic, harmless, green, environmentally friendly, degradable, and imparts superior properties to paper, effectively expanding its scope of application.
[0074] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A coating with high heat seal strength and high barrier properties, Features: The preparation method of the coating with high heat-sealing strength and high barrier performance comprises the following steps: After the collagen fibers are heated and dissolved, glutaraldehyde is added thereto for cross-linking. The amount of glutaraldehyde added is 1%-10% of the mass of the collagen fibers. The mixture is stirred and reacted for 0.5-1 h. After the reaction is completed, gelatinized starch, nanocellulose and sodium alginate are added in sequence, and stirred and mixed under heating conditions; the amount of starch added is 20%-50% of the mass of the collagen fibers, the amount of nanocellulose added is 10%-20% of the mass of the collagen fibers; the amount of sodium alginate added is 3%-10% of the mass of the collagen fibers; Finally, add calcium chloride, the amount of which is 1%-5% of the mass of the sodium alginate, and stir the reaction for 1-1.5 hours to obtain the coating; The method also includes the steps of uniformly coating the prepared coating on paper and drying the paper to prepare the packaging paper; The temperature for heating and dissolving collagen fibers is 40-65°C; In the process of sequentially adding starch, nanocellulose and sodium alginate to the collagen fibers, each time a substance is added, it is first mixed evenly before adding the next substance; The addition of gelatinized starch and nanocellulose improves the barrier and mechanical properties of the film through intermolecular physical effects; the double network structure formed by cross-linking between sodium alginate and calcium chloride is used to enhance the mechanical and barrier properties of the film.
2. The high heat seal strength and high barrier performance coating according to claim 1, Features: The amount of glutaraldehyde added is 5%-8% of the mass of collagen fibers.
3. The high heat seal strength and high barrier performance coating according to claim 1, Features: The amount of starch added is 30%-40% of the mass of the collagen fibers.
4. The high heat seal strength and high barrier performance coating according to claim 1, Features: During the starch addition process, the temperature of the collagen fibers is 35-45°C.
5. The high heat seal strength and high barrier performance coating according to claim 1, Features: The starch is selected from one of corn starch, pea starch or cationic tapioca starch or a combination thereof.
6. The high heat seal strength and high barrier performance coating according to claim 1, Features: The amount of nanocellulose added is 15%-18% of the collagen fiber, the stirring temperature is 35-45°C, and the stirring time is 20-30 min.
7. The high heat seal strength and high barrier performance coating according to claim 1, Features: The specification of the coating rod is 5-50 μm, and the coating amount is 1-10 g / m 2 .
8. The high heat seal strength and high barrier performance coating according to claim 7, Features: The specification of the coating rod is 5-20 μm, and the coating amount is 2-5 g / m 2 .
9. A food packaging paper, Features: A packaging film is coated on the paper base, and the packaging film is prepared by coating the coating according to claim 1 and then drying it.