Ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grain, preparation method and application thereof

By amino modification and ethylenediaminetetraacetic acid grafting cerium oxide composite abrasive particles with excellent dispersion and wetting properties, the cerium oxide abrasive particles were prepared, and the cerium oxide abrasive particles were solved The problems of easy agglomeration and polishing liquid storage conditions have achieved efficient and precise glass surface processing and extended the service life of polishing liquid.

CN116285895BActive Publication Date: 2024-11-12SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310222660.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-12
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

The existing cerium oxide abrasive particles are prone to agglomeration in the polishing liquid, resulting in low processing quality on the glass surface, and the storage conditions of the polishing liquid are harsh and limited in use, making it difficult to meet the processing needs of high concentration and high efficiency.

Method used

By amino modification of cerium oxide abrasive particles and ethylenediaminetetraacetic acid grafting treatment, ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive particles were prepared to improve their dispersion and wetting properties in the polishing liquid. Anhydrous toluene and ethanol/acetic acid mixed solution were treated to form composite abrasive particles with carboxyl terminal groups.

Benefits of technology

It significantly improves the accuracy and efficiency of glass surface processing, reduces surface roughness, improves material removal rate and polishing rate, extends the service life of the polishing liquid, and improves the dispersion and storage conditions of abrasive particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285895B_ABST
    Figure CN116285895B_ABST
Patent Text Reader

Abstract

The invention discloses an ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive, a preparation method and application thereof, and relates to the technical field of polishing abrasive production. Firstly, pure cerium oxide abrasive is subjected to amino modification treatment to obtain amino-modified cerium oxide abrasive, and then ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive is subjected to ethylenediaminetetraacetic acid grafting treatment to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive. The polishing liquid prepared by using the composite abrasive has excellent dispersibility and significantly reduces hard agglomeration. When applied to glass polishing, the polishing efficiency and polishing quality can be significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polishing abrasive production, in particular to ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains, a preparation method and application thereof. Background Art

[0002] As the most common inorganic material, glass has a long history of industrialization and commercialization. With the advancement of science and technology, while promoting the transformation and upgrading of the traditional glass industry, the application scope of glass materials is also expanding, becoming an important material in the fields of information display, aerospace, new energy, etc. At the same time, with the development of applications in these advanced fields, more stringent requirements are put forward for the surface processing of modern glass materials.

[0003] In modern manufacturing industry, chemical mechanical polishing (CMP) is often used for surface processing of glass. In CMP, abrasive grains have a crucial influence on surface quality and material removal rate. Among many abrasive grains, rare earth oxide cerium oxide (CeO2) has special reaction characteristics with glass materials, so it has a high material removal rate (MRR), making it the best abrasive grain for polishing glass.

[0004] When cerium oxide abrasive powder is configured into a polishing liquid, the finer the particle size, the easier it is to agglomerate together to form large agglomerates. When used for polishing the glass surface, large agglomerates will scratch the glass surface, resulting in low surface processing quality of the workpiece. The cerium oxide polishing powder on the market can generally be used for rough processing, but when fine processing is required, the current cerium oxide polishing powder needs to be pre-dispersed in the polishing liquid, and a dispersant must be added to break up the agglomeration process to reduce the content of large agglomerates in the polishing liquid, thereby improving the polishing quality.

[0005] Polishing fluid is generally recommended to be used within six months, and its shelf life is short. Sometimes, due to additives, the storage conditions are harsh, such as light avoidance and temperature restrictions, to prevent the slurry from deteriorating. When in use, the concentration is fixed. When high-concentration polishing fluid is required under certain special working conditions, its use is limited and it is necessary to re-purchase high-concentration polishing fluid. Summary of the invention

[0006] In order to solve the problems of the prior art, the purpose of the present invention is to overcome the shortcomings of the existing technology and provide an ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive, a preparation method and an application thereof. Compared with commercially available cerium oxide abrasives, the composite abrasive is easier to store and use, and has better dispersibility after being configured into a polishing liquid. When used in the field of glass surface processing, it can significantly improve the processing efficiency and surface processing quality to meet the increasingly stringent needs of glass finishing.

[0007] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0008] A method for preparing ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive particles comprises the following steps:

[0009] S1, performing amino modification treatment on pure cerium oxide abrasive grains to obtain amino modified cerium oxide abrasive grains;

[0010] S2, performing ethylenediaminetetraacetic acid grafting treatment on the amino-modified cerium oxide abrasive to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive.

[0011] Preferably, step S1 further comprises:

[0012] S11, adding the pure cerium oxide abrasive grains into anhydrous toluene, mixing them evenly, and obtaining a cerium oxide suspension;

[0013] S12, adding APTES to the cerium oxide suspension, subjecting the suspension to a constant temperature bath treatment, and keeping the temperature at 78° C. for 8 hours to obtain a first sample suspension;

[0014] S13, performing solid-liquid separation on the first sample suspension to obtain a first precipitated sample;

[0015] S14, washing the first precipitated sample to obtain a first washed sample;

[0016] S15, drying the first washed sample to obtain the amino-modified cerium oxide abrasive.

[0017] Preferably, step S2 further comprises:

[0018] S21, adding the amino-modified cerium oxide abrasive to an ethanol / acetic acid mixed solution, mixing evenly, to obtain an amino-modified cerium oxide suspension;

[0019] S22, quickly adding EDTA to the amino-modified cerium oxide suspension, performing a constant temperature bath treatment, and keeping the temperature at 50° C. for 6 hours to obtain a second sample suspension;

[0020] S23, performing solid-liquid separation on the second sample suspension to obtain a second precipitated sample;

[0021] S24, washing the second precipitated sample to obtain a second washed sample;

[0022] S25, drying the second washed sample to obtain the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive.

[0023] Further preferably, in step S11, the uniform mixing treatment is performed by first performing ultrasonic treatment and then performing magnetic stirring.

[0024] Further preferably, in step S12, the constant temperature bath adopts an oil bath for heating and heat preservation.

[0025] Further preferably, in step S22, the constant temperature bath is heated and kept warm by a water bath, and the amino-modified cerium oxide suspension is stirred during the water bath.

[0026] More preferably, between step S21 and step S22, the amino-modified cerium oxide suspension is subjected to a constant temperature bath heating treatment at a temperature of 50°C.

[0027] Further preferably, in step S13 or S23, the solid-liquid separation is performed by centrifugation.

[0028] Further preferably, in step S14 or S24, the washing treatment is firstly washed multiple times with deionized water, and then washed multiple times with ethanol.

[0029] Further preferably, in step S15 or S25, the drying process is performed in an air environment.

[0030] An ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive prepared by the above-mentioned preparation method of ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive, the surface of the cerium oxide abrasive is grafted with ethylenediaminetetraacetic acid, the surface has groups such as -C=O, -CO, and a carboxyl-containing group as the terminal group.

[0031] The invention discloses an ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid, which is prepared by adding the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive into deionized water.

[0032] The invention discloses an application of an ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid. The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid is used in the field of glass polishing. The carboxyl group is used as the terminal group to enhance the wetting performance of the glass substrate, which can significantly improve the material removal rate, reduce the surface roughness of the glass workpiece, and achieve the purpose of high-efficiency and high-precision processing.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The invention prepares ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains by a simple two-step method. A silane coupling agent γ-aminopropyltriethoxysilane (APTES) in anhydrous toluene acts on cerium oxide through a chemical bond, so that the amino group is exposed on the outer surface. Then, the reaction activity of the amino group is used in an ethanol / acetic acid mixed solution to cause a condensation reaction with the carboxyl group of ethylenediaminetetraacetic acid to prepare ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains. The novel abrasive grain preparation method is simple and can be scaled up for industrial production.

[0035] The ethylenediaminetetraacetic acid grafted cerium oxide abrasive prepared by the present invention can efficiently finish glass materials due to the reduction of hard agglomeration, thereby achieving the purpose of efficient finishing. The surface roughness of the glass reaches 1.2nm, which is 21.57% higher than the processing accuracy of commercially available cerium oxide abrasives.

[0036] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains prepared by the present invention have excellent dispersibility in the polishing liquid, and the hard precipitation is significantly reduced, the hard agglomeration between the abrasive grains is improved, and the dispersibility is significantly improved.

[0037] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive prepared by the present invention uses a carboxyl group as the terminal group, so that its wetting performance on the glass substrate is enhanced, and the surface tension between the polishing liquid and the glass substrate is also reduced, which is conducive to the polishing liquid quickly wetting the surface of the glass substrate, thereby improving its polishing rate, and can significantly improve the material removal rate and the polishing efficiency. Compared with conventional commercially available cerium oxide abrasives, the polishing rate of the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive can be increased by a maximum of 42.25%.

[0038] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid prepared by the present invention is applied to chemical mechanical polishing of glass materials, and can effectively improve the polishing efficiency of substrate glass and reduce the surface roughness of substrate glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The infrared spectra of pure cerium oxide, amino-modified cerium oxide abrasive and ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive of Example 2 of the present invention;

[0040] Figure 2 The TOF-SIMS graphs are of the pure cerium oxide, the amino-modified cerium oxide abrasive and the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive of Example 2 of the present invention. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] For ease of understanding, let us first explain the English terms mentioned below:

[0043] APTES: Its chemical name is γ-aminopropyltriethoxysilane.

[0044] EDTA: Its chemical name is ethylenediaminetetraacetic acid.

[0045] MRR: Abbreviation for Material Removal Rate.

[0046] Sa: Abbreviation for surface roughness.

[0047] CeO2: Cerium oxide.

[0048] CeO2-NH2: Abbreviation for amino-modified cerium oxide abrasive.

[0049] CeO2-EDTA: abbreviation of ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive.

[0050] The present invention provides the following technical solution: a method for preparing ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive particles, comprising the following steps:

[0051] S1, performing amino modification treatment on pure cerium oxide abrasive grains to obtain amino modified cerium oxide abrasive grains;

[0052] S2, subjecting the amino-modified cerium oxide abrasive to ethylenediaminetetraacetic acid grafting treatment to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive.

[0053] Furthermore, step S1 includes:

[0054] S11, adding pure cerium oxide abrasive grains into anhydrous toluene and mixing them evenly to obtain a cerium oxide suspension;

[0055] S12, adding APTES to the cerium oxide suspension, subjecting the suspension to a constant temperature bath treatment, and maintaining the temperature at 78° C. for 8 hours to obtain a first sample suspension;

[0056] S13, performing solid-liquid separation on the first sample suspension obtained in step S12 to obtain a first precipitated sample;

[0057] S14, washing the first precipitated sample obtained in step S13 to obtain a first washed sample;

[0058] S15, drying the first washed sample to obtain amino-modified cerium oxide abrasive grains.

[0059] Furthermore, step S2 includes:

[0060] S21, adding the amino-modified cerium oxide abrasive to the ethanol / acetic acid mixed solution, mixing evenly, to obtain an amino-modified cerium oxide suspension;

[0061] S22, quickly adding EDTA to the amino-modified cerium oxide suspension, performing a constant temperature bath treatment, and keeping the temperature at 50° C. for 6 hours to obtain a second sample suspension;

[0062] S23, performing solid-liquid separation on the second sample suspension obtained in step S22 to obtain a second precipitated sample;

[0063] S24, washing the second precipitated sample obtained in step S24 to obtain a second washed sample;

[0064] S25, drying the second washed sample to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains.

[0065] Furthermore, in step S11, ultrasonic treatment is first performed and then magnetic stirring is used to mix uniformly.

[0066] Furthermore, in step S12, the constant temperature bath uses an oil bath for heating and heat preservation.

[0067] Furthermore, in step S22, the constant temperature bath is heated and kept warm by a water bath, and the amino-modified cerium oxide suspension is stirred during the water bath.

[0068] Furthermore, between step S21 and step S22, the amino-modified cerium oxide suspension is subjected to a constant temperature bath heating treatment at a temperature of 50°C.

[0069] Furthermore, in step S13 or S23, solid-liquid separation is performed by centrifugation.

[0070] Furthermore, in step S14 or S24, the washing is first performed multiple times with deionized water and then multiple times with ethanol to remove substances such as APTES and anhydrous toluene remaining on the surface of the precipitated sample.

[0071] Furthermore, in step S1, the ratio of each material is cerium oxide: anhydrous toluene: APTES = 10:40:3.

[0072] Furthermore, in step S2, the ratio of the materials is amino-modified cerium oxide: ethanol: acetic acid: EDTA = 24: 240: 240: 1-4.

[0073] It should be further explained that the ethylenediaminetetraacetic acid-grafted cerium oxide composite abrasive prepared in the present invention only needs to be manually ground in a mortar after being dried in step S25 and can be stored for later use.

[0074] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains prepared by the above-mentioned technical scheme of the preparation method of ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grains have the following technical characteristics:

[0075] The surface of the cerium oxide abrasive is grafted with ethylenediaminetetraacetic acid, and has groups such as -C=O, -CO, and carboxyl-containing groups such as C2OH, CO2H, C2O2H3, C3H6NO2, etc.

[0076] The present invention provides a technical solution: an application of ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive particles, comprising the following steps:

[0077] The oxalic acid tetraacetic acid grafted cerium oxide composite abrasive grains are added into deionized water to prepare the oxalic acid tetraacetic acid grafted cerium oxide composite abrasive grain polishing liquid.

[0078] Embodiment 1:

[0079] (1) adding 60 g of pure cerium oxide abrasive particles with an average particle size of 1 μm to 240 g of anhydrous toluene, ultrasonicating for 10 min, and then magnetically stirring for 10 min to obtain a cerium oxide suspension;

[0080] (2) 18 g of APTES was added to the cerium oxide suspension, placed in a constant temperature oil bath environment, and reacted for 8 hours at 78° C. to obtain a first sample suspension. In this embodiment, an oil bath was used for heating and heat preservation. The sample container was sealed during heating, and reflux condensation was performed after heating. It should be noted that a water bath can also be used for constant temperature bathing in this step. However, considering that the evaporation of water is large at 78° C., when water evaporates excessively and is not replenished in time, uneven heating occurs. Therefore, an oil bath was used in this embodiment to improve the stability of the reaction.

[0081] (3) centrifuging the first sample suspension at 5000 rpm for 5 min to obtain a first precipitated sample;

[0082] (4) The first precipitated sample is washed twice with deionized water and ethanol respectively to remove substances such as APTES and anhydrous toluene, thereby obtaining a first washed sample. It should be noted that the initial washing liquid is yellow, and the supernatant is colorless and transparent after the washing is completed. In actual operation, the washing liquid and the number of washes can be determined according to the liquid state during the actual washing.

[0083] (5) drying the first washed sample at 60° C. for 8 h to obtain amino-modified cerium oxide abrasive particles;

[0084] (6) preparing an ethanol / acetic acid mixed solution by mixing ethanol and acetic acid in a mass ratio of 1:1;

[0085] (7) 6 g of amino-modified cerium oxide abrasive was placed in 120 g of ethanol / acetic acid mixed solution, ultrasonicated for 10 min, and magnetically stirred for 10 min to mix evenly to obtain an amino-modified cerium oxide suspension;

[0086] (8) placing the amino-modified cerium oxide suspension in a water bath and heating it at a temperature of 50° C.

[0087] (9) 0.25 g of ethylenediaminetetraacetic acid was quickly added to the amino-modified cerium oxide suspension, and the mixture was stirred continuously. The mixture was kept in a water bath at 50° C. for 6 h to obtain a second sample suspension. It should be noted that magnetic stirring was used for stirring in this embodiment. In practice, other stirring methods may be used, such as manual stirring.

[0088] (10) centrifuging the second sample suspension at 5000 rpm for 5 min to obtain a second precipitate sample;

[0089] (11) The second precipitated sample is washed twice with deionized water and ethanol respectively to remove excess EDTA and other substances, thereby obtaining a second washed sample. It should be noted that the washing liquid is turbid at the beginning, and the supernatant is clear and transparent after the washing is completed. In actual operation, the washing liquid and the number of washing times can be determined according to the liquid state during the actual washing;

[0090] (12) The second washed sample was dried at 60° C. for 8 h to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive particles.

[0091] (13) Add ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive into deionized water to prepare ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid, wherein the mass fraction of the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive is 2%.

[0092] It should be noted that: ① In this embodiment, anhydrous toluene can be replaced by ethanol, water, or a mixture of ethanol and water, etc., but by comparison, it is found that the number of amino groups of the modified cerium oxide abrasive obtained after treatment with anhydrous toluene is greater, and under the condition of anhydrous toluene, the binding of APTES on the surface of cerium oxide abrasive is often a monolayer reaction, and the self-condensation of APTES is reduced; ② In this embodiment, both ultrasound and magnetic stirring are methods for uniform mixing. In actual operation, ultrasonic dispersion method or magnetic stirring method or a combination of the two can be used, or other mixing methods can be used to make the cerium oxide abrasive uniformly dispersed in anhydrous toluene. It is noted that, in practice, the duration of ultrasonic and magnetic stirring can be appropriately adjusted according to the particle size and quantity of the material; ③ In this embodiment, centrifugal separation is a method of solid-liquid separation. In actual operation, the speed and time can be adjusted according to the different particle sizes and quantities of the materials; ④ In this embodiment, the drying method is drying in an air environment, using 60°C and 8h drying conditions, but in actual operation, according to the physical and chemical properties of the material, it can be known that the material can be dried at room temperature to 120°C without causing changes in the properties of the material, and the drying time can also be appropriately adjusted with changes in the quantity of the material and other conditions. ⑤ In this embodiment, the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive is configured into a polishing liquid with a mass fraction of 2%, but in actual operation, the concentration of the abrasive can be changed to adjust the polishing rate.

[0093] Embodiment 2:

[0094] This embodiment is basically the same as Embodiment 1, except that:

[0095] In this embodiment, steps (1) to (8) are the same as those described in Embodiment 1;

[0096] (9) quickly adding 0.5 g of EDTA to the amino-modified cerium oxide suspension, continuously stirring, and maintaining the suspension at 50° C. in a water bath for 6 h to obtain a second sample suspension;

[0097] The subsequent steps are the same as steps (10) to (13) described in Example 1.

[0098] Embodiment 3:

[0099] This embodiment is basically the same as Embodiment 1, except that:

[0100] In this embodiment, steps (1) to (8) are the same as those described in Embodiment 1;

[0101] (9) quickly adding 0.75 g of EDTA to the amino-modified cerium oxide suspension, continuously stirring, and maintaining the suspension at 50° C. in a water bath for 6 h to obtain a second sample suspension;

[0102] The subsequent steps are the same as steps (10) to (13) described in Example 1.

[0103] Embodiment 4:

[0104] This embodiment is basically the same as Embodiment 1, except that:

[0105] In this embodiment, steps (1) to (8) are the same as those described in Embodiment 1;

[0106] (9) quickly adding 1 g of EDTA to the amino-modified cerium oxide suspension, continuously stirring, and maintaining the suspension at 50° C. in a water bath for 6 h to obtain a second sample suspension;

[0107] The subsequent steps are the same as steps (10) to (13) described in Example 1.

[0108] Embodiment 5:

[0109] This embodiment is basically the same as Embodiment 1, except that:

[0110] In this embodiment, steps (1) to (8) are the same as those described in Embodiment 1;

[0111] (9) 1.25 g of EDTA was quickly added to the amino-modified cerium oxide suspension, and the mixture was stirred continuously and kept in a water bath at 50° C. for 6 h to obtain a second sample suspension;

[0112] The subsequent steps are the same as steps (10) to (13) described in Example 1.

[0113] Comparative Example 1:

[0114] Pure cerium oxide abrasive grains that have not been modified are added into deionized water to prepare a cerium oxide polishing liquid, wherein the mass fraction of the cerium oxide abrasive grains is 2%.

[0115] Comparative Example 2:

[0116] In this comparative example, the steps (1) to (5) described in Example 1 were the same as those to obtain amino-modified cerium oxide abrasive grains;

[0117] Amino-modified cerium oxide abrasive grains were added into deionized water to prepare amino-modified cerium oxide polishing liquid, wherein the mass fraction of the amino-modified cerium oxide abrasive grains was 2%.

[0118] Polishing experiments were carried out using the polishing liquids prepared in Examples 1-5 and Comparative Examples 1-2, as follows:

[0119] Polishing object: ordinary soda-lime glass, Sa=1.94nm;

[0120] The polishing conditions of the polishing test are as follows:

[0121] Polishing machine: UNIPOL-1000s automatic pressure grinding and polishing machine;

[0122] Workpiece: Ordinary soda-lime glass sheet with a diameter of 50 mm and a thickness of 2 mm;

[0123] Polishing pad: polyurethane polishing pad;

[0124] Polishing pressure: 4kg;

[0125] Upper plate speed: 30rpm;

[0126] Lower plate speed: 60rpm;

[0127] Polishing time: 30min;

[0128] After polishing, the ordinary soda-lime glass sheet was washed and dried in the order of cleaning liquid, deionized water, and ethanol, and the mass of the substrate glass sheet before and after polishing was weighed with a precision analytical balance to calculate the material removal rate MRR. In addition, the surface roughness (Sa) of the substrate glass sheet before and after polishing measured by a 3D surface profiler was 0.5% in step accuracy, 0.1% in step repeatability, 0.1nm in vertical resolution, 0.14nm in lateral resolution at most, and 0.1nm-34mm in Z-direction scanning range.

[0129] The polishing effects of the polishing liquids prepared in the embodiments and comparative examples on ordinary soda-lime glass sheets are shown in Table 1, wherein: the EDTA ratio (wt%) is the ratio of the mass of EDTA added in the preparation method of each embodiment to the mass of the amino-modified cerium oxide abrasive grains; compared with Comparative Example 1, Wherein x=1, 2, 3, 4 or 5; Compared with Comparative Example 1, Where x=1, 2, 3, 4 or 5.

[0130] Table 1. Polishing effect of the polishing liquid in each embodiment of the present invention and the comparative example on the substrate glass

[0131]

[0132]

[0133] As can be seen from Table 1, compared with the unmodified pure cerium oxide abrasive (Comparative Example 1) and the amino-modified cerium oxide abrasive (Comparative Example 2), the material removal rates of the polishing liquids of Examples 1-4 are significantly increased, among which the material removal rate of the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive with an EDTA content of 8.33% in Example 2 is the most significantly improved compared with the commercially available cerium oxide abrasive in Comparative Example 1, with an MRR increase of 42.25%, and a higher quality smooth surface (Sa = 1.31nm) is obtained. This proves that grafting ethylenediaminetetraacetic acid can significantly increase the material removal rate of cerium oxide abrasives and improve the surface quality of the workpiece. However, if the ethylenediaminetetraacetic acid grafting rate is too high, such as in Example 5, the abrasive removal rate will be greatly reduced, and the higher chemical reaction activity will enhance the reaction between the composite abrasive and the workpiece surface, thereby resulting in a decrease in surface quality. Therefore, the EDTA ratio (wt%) is between 4.17% and 16.67%, that is, the mass ratio of EDTA to the amino-modified cerium oxide abrasive is between 1 and 4:24, preferably 1 to 3:24, and more preferably 1:12.

[0134] from Figure 1 As can be seen, there are four obvious characteristic absorption peaks (1640cm -1 、1460cm -1 、1004cm -1 and 914cm -1 ) is the peak position of CeO2; on the curve corresponding to CeO2-NH2, it is located at 3443cm -1 The characteristic absorption peak near 3443 cm -1 The intensity of the broad peak at 2930 cm-1 is significantly enhanced, which is due to the increase of hydroxyl groups on the abrasive surface and the superposition of amino peaks. -1 、2880cm -1 、1690cm -1 、1490cm -1 The characteristic absorption peaks corresponding to -CH2 symmetric stretching, -CH2 asymmetric stretching, -C=O, and -CN appeared at 3443cm-1. In contrast, the curve of CeO2-EDTA showed a peak at 3443cm-1 after the amino-modified cerium oxide abrasive was grafted with EDTA. -1 The broad peak at 1407 cm-1 is weakened, which is due to the combination of amino groups with EDTA, resulting in a decrease in the number of amino groups. The characteristic peak of -C=O is enhanced, at 1407 cm-1. -1 、1316cm -1 The characteristic absorption peak of -CO appears at , proving that the grafting of EDTA is successful.

[0135] from Figure 2 It can be seen that in the TOF-SIMS analysis results of CeO2, CeO2-NH2 and CeO2-EDTA, in the corresponding spectrum of CeO2-NH2, CN, CNO, Si2O5H and Si3O7H fragment ions in APTES appeared, and special ion fragments that were obviously different from pure cerium oxide appeared at the mass-to-charge ratio m / z=127, which indicated that APTES was successfully bound to the surface of cerium oxide; in addition, some other trace fragment ions, such as C2OH, CO2H, C2O2H3, C3H6NO2, etc., were seen in the corresponding spectrum of CeO2-EDTA, which proved that CeO2-NH2 successfully reacted with EDTA to expose the carboxyl group outside the cerium oxide.

[0136] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive prepared by the present invention has better dispersibility, which is mainly reflected in: the embodiment 1-5 and the comparative example 1-2 are shaken and evenly tested, that is, each polishing liquid sample is in a precipitated state, and then shaken. After shaking for 5 times, it can be seen that the CeO2-EDTA abrasive in the polishing liquid of the embodiment 1-5 has been evenly dispersed, while after shaking for 5 times, there is still obvious hard precipitation attached to the bottom of the glass bottle in the comparative example 1-2, and the comparative example 1 needs to be shaken for 20 times before the hard precipitation at the bottom disappears. It can be seen that the dispersibility of the CeO2-EDTA abrasive after ethylenediaminetetraacetic acid grafting in water is improved.

[0137] The ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive prepared by the present invention has good dispersibility, which is mainly reflected in: a precipitation experiment is carried out on Examples 1-5 and Comparative Examples 1-2, that is, each polishing liquid sample is in a uniformly dispersed state, and is allowed to stand at the same time to prevent that there is no obvious difference in dispersibility after 12 hours, and after 24 hours and 48 hours, the sedimentation of Examples 1-3 is still small.

[0138] It should be noted that in the present invention, cerium oxide abrasives with an average particle size of 1 micron are selected as raw materials for grafting treatment, but in practice we know that the particle size range of cerium oxide abrasives includes nanometers, micrometers, etc., and can all be used as abrasives. The ethylenediamine grafted cerium oxide composite abrasives described in the present invention, their preparation method and particle size ranges of nanometers and micrometers are also applicable, but it is necessary to make appropriate adjustments in the material ratio and process parameters to obtain suitable grafting effect and polishing effect of cerium oxide abrasives.

[0139] In summary: compared with conventional commercially available pure cerium oxide abrasives, the agglomeration of the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasives in the polishing liquid is improved, so that the dispersion stability is improved. At the same time, the cerium oxide composite abrasives obtained after ethylenediaminetetraacetic acid grafting have carboxyl groups as terminal groups, which enhances their wetting properties on the glass substrate, can significantly improve the material removal rate, and achieve the purpose of efficient finishing.

[0140] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the attached embodiments and their equivalents.

Claims

1. A method for preparing ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive, characterized in that: The following steps are involved: S1, performing amino modification treatment on pure cerium oxide abrasive grains to obtain amino modified cerium oxide abrasive grains; S2, performing ethylenediaminetetraacetic acid grafting treatment on the amino-modified cerium oxide abrasive to obtain ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive; The step S1 further comprises: adding the pure cerium oxide abrasive grains into anhydrous toluene, mixing them uniformly to obtain a cerium oxide suspension, adding APTES into the cerium oxide suspension, subjecting the suspension to a constant temperature bath treatment, and keeping the temperature at 78° C. for 8 hours to obtain a first sample suspension, subjecting the first sample suspension to solid-liquid separation to obtain a first precipitated sample, subjecting the first precipitated sample to a washing treatment to obtain a first washed sample, and subjecting the first washed sample to a drying treatment to obtain the amino-modified cerium oxide abrasive grains; B. The S2 step also includes: adding the amino-modified cerium oxide abrasive to an ethanol / acetic acid mixed solution, mixing evenly to obtain an amino-modified cerium oxide suspension, quickly adding EDTA to the amino-modified cerium oxide suspension, subjecting it to a constant temperature bath treatment, and keeping it warm at 50°C for 6 hours to obtain a second sample suspension, subjecting the second sample suspension to solid-liquid separation to obtain a second precipitated sample, washing the second precipitated sample to obtain a second washed sample, and drying the second washed sample to obtain the ethylenediaminetetraacetic acid-grafted cerium oxide composite abrasive, wherein the amino-modified cerium oxide abrasive: ethanol: acetic acid: EDTA = 24:240:240:(1~4).

2. The method for preparing the composite abrasive grains of ethylenediaminetetraacetic acid grafted cerium oxide according to claim 1, characterized in that: In the step S1, the uniform mixing is performed by first performing ultrasonic treatment and then performing magnetic stirring.

3. The method for preparing the composite abrasive grains of ethylenediaminetetraacetic acid grafted cerium oxide according to claim 1, characterized in that: The constant temperature bath in step S1 is heated and kept warm by an oil bath.

4. The method for preparing the composite abrasive grains of ethylenediaminetetraacetic acid grafted cerium oxide according to claim 1, characterized in that: In the step S2, the constant temperature bath is heated and kept warm by a water bath, and the amino-modified cerium oxide suspension is stirred during the water bath.

5. The method for preparing the composite abrasive grains of ethylenediaminetetraacetic acid grafted cerium oxide according to claim 1, characterized in that: The step S2 also includes firstly subjecting the amino-modified cerium oxide suspension to a constant temperature bath heating treatment at a temperature of 50° C., and then rapidly adding EDTA into the amino-modified cerium oxide suspension.

6. The method for preparing the composite abrasive grains of ethylenediaminetetraacetic acid grafted cerium oxide according to claim 1, characterized in that: The solid-liquid separation is performed by centrifugation, the washing treatment is firstly performed multiple times with deionized water, and then multiple times with ethanol, and the drying treatment is performed in an air environment.

7. An ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grain, prepared by the preparation method of ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive grain according to any one of claims 1 to 6, characterized in that: The surface of the cerium oxide composite abrasive grain is grafted with ethylenediaminetetraacetic acid, has -C=O and -CO groups on the surface, and has a carboxyl-containing group as a terminal group.

8. An ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive polishing liquid, prepared using the ethylenediaminetetraacetic acid grafted cerium oxide composite abrasive according to claim 7, characterized in that: The composite abrasive grains grafted with ethylenediaminetetraacetic acid and cerium oxide are added into deionized water for preparation.