A method for adding rare earth alloy to LF refining furnace
By controlling the low oxidation and deep desulfurization process in the LF refining furnace, combined with soft blowing wire feeding technology, the yield rate of rare earth alloys and the castability of the casting machine are improved, and the problem of poor treatment effect of rare earth steel is solved. Efficient utilization of rare earth resources.
Patent Information
- Application Number
- CN202310083701.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-08
AI Technical Summary
The existing technology cannot effectively improve the yield rate of rare earth alloys and the pourability of molten steel, resulting in poor treatment effects of rare earth steel and affecting the economic utilization of resources.
Using the LF refining furnace method, by controlling the low oxidation of molten steel and steel slag, deep desulfurization process and soft blowing wire feeding technology, the yield rate of rare earth alloys and the continuous casting stability of the casting machine are improved to ensure the content of rare earths in steel and low oxidation of molten steel.
It achieves a high yield of rare earth alloys and good pourability of the casting machine. Rare earth micro-alloyed steel can be continuously poured for 30 furnaces, and rare earth alloyed steel can be continuously cast for 6 furnaces, which reduces production costs.
Smart Images

Figure BDA0004068328490000071 
Figure BDA0004068328490000081
Abstract
Description
Technical Field
[0001] The invention relates to a method for adding rare earth alloy into a LF refining furnace. Background Art
[0002] Rare earth refers to the lanthanide elements of Group IB in the periodic table, as well as scandium and yttrium, which are similar to lanthanide elements in chemical properties, a total of 17 elements. It was discovered by Finnish scholar Johan Gadolin in 1794. At that time, yttrium earth with a mineral composition similar to "soil" was found in Swedish ores, and it was considered rare, so it was named "rare earth" (Baxe Earth). Since then, many similar elements have been discovered one after another, collectively known as rare earths. However, later studies have found that the abundance of rare earths in the earth's crust is much greater than people imagined. For example, cerium is much more abundant than tin, yttrium is more abundant than lead, and even the rare earth elements with the least abundance are more abundant than platinum group elements, indicating that rare earths are not rare. They are not "soil" either, all of them are metal elements. my country is rich in rare earth resources, which is unmatched by any other country in the world. The current proven industrial reserves are 36 million tons, accounting for about 80% of the world's total, and there are many varieties and concentrated distribution. The reserves of the Bayan Obo Mine in Baotou City account for more than 95% of the national reserves. That is why there is a saying that "the world's rare earths are in China, and China's rare earths are in Baotou". Although Baotou Steel has rich rare earth resources, it still lags far behind Wuhan Iron and Steel, Jigang, Benxi Steel and other companies in terms of the variety and treatment effect of rare earth treated steel. How to turn the resource advantage of rare earths into an economic advantage has become an imminent issue.
[0003] A large amount of research and production experience have shown that rare earth elements have an important influence on the structure and mechanical properties of steel and alloys. The rare earth metal content in steel varies greatly due to different steel grades, different smelting methods and different rare earth addition methods, but the low rare earth yield and poor castability of the casting machine are the biggest problems in smelting rare earth steel. How to effectively improve the yield of rare earth alloys and improve the castability of molten steel is the most important problem in current production.
[0004] The invention discloses a method for adding rare earth alloys to an LF refining furnace, and particularly relates to a method for adding rare earth alloys to an LF refining furnace. The method can effectively improve the yield of rare earth alloys, reduce costs, and ensure the castability of a casting machine. The rare earth content added to the steel by the method can reach about 100 ppm, and the castability of the casting machine is good. The continuous casting of rare earth microalloyed steel (rare earth content 10-30 ppm) can reach 30 furnaces, and the continuous casting of rare earth alloyed steel (rare earth content above 30 ppm) can reach 6 furnaces. Summary of the invention
[0005] The purpose of the present invention is to provide a method for adding rare earth alloys to a LF refining furnace, which overcomes the disadvantage that the existing smelting process cannot improve the yield of rare earth alloys, and at the same time, the process also has good effects in reducing costs and ensuring the castability of the casting machine.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A method for adding rare earth alloy to a LF refining furnace of the present invention comprises the following steps:
[0008] S1. Control of low oxidation of molten steel
[0009] The control of low oxidation of molten steel includes two aspects: one is the deoxidation of molten steel, and the other is the deoxidation of slag:
[0010] (1) Slag washing process
[0011] During the steel-making process, the converter slag washing process is adopted. When the molten steel covers the bottom of the tank, micro-carbon aluminum iron is added for deoxidation, and the aluminum content in the molten steel is controlled to 0.060%-0.070%; when the steel is tapped to one-half, 900-1100kg of lime and 250-350kg of slag deoxidizer are added;
[0012] (2) Refining and deoxidation white slag making process
[0013] In the refining and slag-making process, lime, slag deoxidizer and aluminum particles are used to make slag; the slag is added in batches, 700-900kg lime, 150-250kg slag, 150-250kg slag deoxidizer and 40-60kg aluminum particles are added to the first batch of slag, and 400-600kg lime is added to the second batch of slag 5 minutes after adding, and then the amount of lime is added to 2000kg in batches during the heating process; the argon gas is controlled at 350-450L / min during the heating process; aluminum particles and slag deoxidizer are added according to the actual slag conditions throughout the refining process to maintain white slag, and the aluminum content in the steel is controlled at 0.055%-0.065%, the slag basicity is controlled at 5.5-6.5, and the CaO content in the slag is controlled at 55%-62%;
[0014] S2. Refining deep desulfurization process
[0015] On the basis of the previous deoxidation and white slag making, the temperature of molten steel is heated to 1550-1650℃, and deep desulfurization of molten steel is started; the argon gas is adjusted to 750-850L / min of double lines for large argon stirring desulfurization, and the color change of slag is observed during the desulfurization stirring process, and slag deoxidizer is added to maintain the low oxidation of slag; the goal is to reduce the sulfur content in molten steel to 0.0015%; 25-35kg of aluminum particles and 80-120kg of slag deoxidizer are added in the subsequent heating to keep the white slag to avoid heating back oxygen; large argon stirring is strictly prohibited after desulfurization is completed;
[0016] S3, Refining and Wire Feeding Process
[0017] In order to reduce the secondary oxidation of molten steel during wire feeding, a soft blowing wire feeding process is adopted; the wire feeding argon gas is set to double-wire 45-55L / min, the wire feeding speed is set to 1.9-2.1m / s, and the feeding calcium wire amount is set to 280-320m;
[0018] S4, rare earth addition process
[0019] After wire feeding, soft blowing is started with a double-line argon flow rate of 25-35L / min. After soft blowing for 2-4 minutes, when the slag liquid surface begins to crust, rare earth alloy is added. After adding the alloy, the soft blowing state is maintained for 3-7 minutes.
[0020] Furthermore, in said (1): when the steel is tapped to half, 1000 kg of lime and 300 kg of slag deoxidizer are added.
[0021] Furthermore, 800 kg of lime, 200 kg of slag, 200 kg of slag deoxidizer and 50 kg of aluminum particles were added to the first batch of slag.
[0022] Furthermore, 500 kg of lime was added to the second batch of slag.
[0023] Furthermore, the argon gas during the heating process was controlled to 400 L / min.
[0024] Furthermore, based on the previous deoxidation and white slag making, the molten steel temperature is heated to 1600°C.
[0025] Furthermore, the argon gas is adjusted to 800 L / min in dual lines for large argon stirring desulfurization.
[0026] Furthermore, in S2, 30 kg of aluminum particles and 100 kg of slag deoxidizer are added during subsequent heating to keep the slag white and avoid heating and reoxidation.
[0027] Furthermore, in S3, the wire feeding argon gas is set to double wire 50L / min, the wire feeding speed is set to 2m / s, and the amount of calcium wire fed is set to 300m.
[0028] Furthermore, in S4, soft blowing is started after wire feeding with a double-line argon flow rate of 30 L / min. After soft blowing for 3 minutes, rare earth alloy is added after the slag liquid surface begins to crust. After the alloy is added, the soft blowing state is maintained for 5 minutes.
[0029] Compared with the prior art, the beneficial technical effects of the present invention are:
[0030] The LF refining furnace uses a traditional deoxidation method to add rare earth alloys. The aluminum content in the molten steel after the converter tapping is low, the lime and slag deoxidizers cannot be well mixed with the molten steel, and the refining LF furnace cannot keep the white slag throughout the whole process, resulting in strong oxidation of the molten steel and slag, which affects the yield of rare earth alloys and the stability of continuous casting of the casting machine. The present invention successfully ensures the low oxidation of molten steel and improves the yield of rare earth alloys and the stability of continuous casting of the casting machine by increasing the aluminum content after the converter tapping and controlling the white slag throughout the refining LF furnace.
[0031] Traditional LF desulfurization technology mainly focuses on the effect of the amount of argon in steel on the desulfurization reaction. It often uses methods such as large argon stirring, which takes a long time and makes the molten steel easy to re-oxygenate in the later stage. In terms of the temperature of the molten steel, stirring and desulfurization are often carried out directly after the slag is melted. The molten steel is not at a suitable desulfurization temperature, resulting in a slow desulfurization rate. During the stirring process, the slag deoxidizer is not added in time according to the color of the slag. After the desulfurization is completed, the slag deoxidizer is not added in time during heating, causing the molten steel to be subjected to secondary oxidation, which affects the yield of rare earth alloys. The present invention controls the temperature of the molten steel during the desulfurization process, shortens the large argon stirring time, and controls the entire steel slag and white slag, thereby accelerating the LF desulfurization reaction rate and improving the yield of rare earth alloys.
[0032] In the traditional refining wire feeding technology, the wire feeding argon is set to double lines at 50-300 / min. The wire feeding argon is large, which easily causes secondary oxidation of molten steel. The present invention reduces secondary oxidation of molten steel during wire feeding by controlling the wire feeding argon size during molten steel feeding, thereby improving the recovery rate of rare earth alloys.
[0033] In the traditional rare earth adding technology, rare earth is added before wire feeding, which will affect the rare earth recovery rate. In the present invention, rare earth alloy is added after soft blowing for 3 minutes after wire feeding and after the slag liquid surface begins to crust, and the soft blowing state is maintained for 5 minutes after the alloy is added, so as to reduce the loss of rare earth caused by wire feeding and improve the recovery rate of rare earth alloy.
[0034] The method can add rare earth content to steel up to about 100ppm, and the caster has good castability. Rare earth micro-alloyed steel (rare earth content 10-30ppm) can be continuously cast for up to 30 furnaces, and rare earth alloyed steel (rare earth content above 30ppm) can be continuously cast for 6 furnaces. DETAILED DESCRIPTION
[0035] A method for adding rare earth alloy to a LF refining furnace, comprising the following steps:
[0036] S1. Control of low oxidation of molten steel
[0037] The control of low oxidation property of molten steel includes two aspects: one is the deoxidation of molten steel, and the other is the deoxidation of slag.
[0038] (1) Slag washing process
[0039] During the steel-making process, the converter slag washing process is adopted. When the molten steel covers the bottom of the tank, micro-carbon aluminum iron is added for deoxidation. The aluminum content in the molten steel is controlled to 0.060%-0.070%. When the steel is tapped to half, 1000kg of lime and 300kg of slag deoxidizer are added.
[0040] (2) Refining and deoxidation white slag making process
[0041] During the refining and slag making process, lime, slag deoxidizer and aluminum particles are used for slag making. The slag is added in batches. The first batch of slag is added with 800kg lime, 200kg slag, 200kg slag deoxidizer and 50kg aluminum particles. After 5 minutes, the second batch of slag is added with 500kg lime. The amount of lime is added to 2000kg in batches during the heating process. The argon gas is controlled at 400L / min during the heating process. Aluminum particles and slag deoxidizer are added according to the actual slag conditions to maintain white slag throughout the refining process, and the aluminum content in the steel is controlled at 0.055%-0.065%, the slag basicity is controlled at 5.5-6.5, and the CaO content in the slag is controlled at 55%-62%.
[0042] S2. Refining deep desulfurization process
[0043] On the basis of the previous deoxidation and white slag making, the temperature of the molten steel is heated to 1600℃, and the deep desulfurization operation of the molten steel is started. The argon gas is adjusted to 800L / min in two lines for large argon stirring desulfurization. During the desulfurization stirring process, the color change of the slag is observed, and slag deoxidizer is added to maintain the low oxidation of the slag. The goal is to reduce the sulfur content in the molten steel to 0.0015%. During the subsequent heating, 30kg of aluminum particles and 100kg of slag deoxidizer are added to keep the white slag to avoid heating back oxygen. Large argon stirring is strictly prohibited after the desulfurization is completed.
[0044] S3, Refining and Wire Feeding Process
[0045] In order to reduce the secondary oxidation of molten steel during wire feeding, a soft blowing wire feeding process is adopted. The wire feeding argon gas is set to double wire 50L / min, the wire feeding speed is set to 2m / s, and the feeding amount of calcium wire is set to 300m.
[0046] S4, rare earth addition process
[0047] After wire feeding, soft blowing is started with a double-line argon flow rate of 30L / min. After soft blowing for 3 minutes, when the slag liquid surface begins to crust, rare earth alloy is added. After adding the alloy, the soft blowing state is maintained for 5 minutes.
[0048] Example 1
[0049] Take the rare earth steel of steel grade Q355C and smelting number 22103558 as an example. The LF furnace in-situ temperature is 1535℃, the in-situ aluminum is 0.061%, the processing time is 73 minutes, the heating time is 23 minutes, the amount of lime added is 2640kg, the amount of modifier added is 745kg, the slag basicity is 5.8, and the CaO content in the slag is 58.42%. The wire feeding argon is double-line 50L / min, the wire feeding speed is 2m / s, and the amount of calcium wire fed is 300m. The double-line argon flow rate of soft blowing is 30L / min. After soft blowing for 3min, the rare earth alloy is added. After adding the alloy, the soft blowing state is maintained for 5min, and the out-of-situ temperature is 1565℃.
[0050] 60 kg of lanthanum-iron alloy was added to this furnace steel, the lanthanum content of the middle package sample was 44 ppm, and the recovery rate of rare earth element lanthanum was 73.33%.
[0051] Example 2
[0052] Take the rare earth steel of steel grade Q355C and smelting number 22103559 as an example. The LF furnace in-situ temperature is 1533℃, the in-situ aluminum is 0.063%, the processing time is 73 minutes, the heating time is 17 minutes, the amount of lime added is 2328kg, the amount of modifier added is 625kg, the slag basicity is 6.1, and the CaO content in the slag is 60.35%. The wire feeding argon is double-line 50L / min, the wire feeding speed is 2m / s, and the amount of calcium wire fed is 300m. The double-line argon flow rate of soft blowing is 30L / min. After soft blowing for 3min, the rare earth alloy is added. After adding the alloy, the soft blowing state is maintained for 5min, and the out-of-situ temperature is 1569℃.
[0053] 90 kg of lanthanum-iron alloy was added to this furnace steel, the lanthanum content of the middle package sample was 56 ppm, and the recovery rate of rare earth element lanthanum was 58.07%.
[0054] Example 3
[0055] Take the rare earth steel of steel grade Q355C and smelting number 22103560 as an example. The LF furnace in-situ temperature is 1522℃, the in-situ aluminum content is 0.066%, the processing time is 79 minutes, the heating time is 22 minutes, the amount of lime added is 2449kg, the amount of modifier added is 940kg, the slag basicity is 6.3, and the CaO content in the slag is 57.86%. The wire feeding argon is double-line 50L / min, the wire feeding speed is 2m / s, and the amount of calcium wire fed is 300m. The double-line argon flow rate of soft blowing is 30L / min. After soft blowing for 3min, the rare earth alloy is added. After adding the alloy, the soft blowing state is maintained for 5min, and the out-of-situ temperature is 1568℃.
[0056] 120 kg of lanthanum-iron alloy was added to this furnace steel, the lanthanum content of the middle package sample was 82 ppm, and the recovery rate of rare earth element lanthanum was 66.97%.
[0057] Table 1 below shows the smelting process data of the three cases.
[0058] Table 1
[0059]
[0060] Table 2 below shows the data of rare earth alloy content in the casting process of three cases
[0061] Table 2
[0062]
[0063] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for adding rare earth alloys to a LF refining furnace, characterized in that: The steps include: S1. Control of low oxidation of molten steel The control of low oxidation of molten steel includes two aspects: one is the deoxidation of molten steel, and the other is the deoxidation of slag: (1) Slag washing process During the steel-making process, the converter slag washing process is adopted. When the molten steel covers the bottom of the tank, micro-carbon aluminum iron is added for deoxidation, and the aluminum content in the molten steel is controlled to 0.060%-0.070%; when the steel is tapped to half, 900-1100kg of lime and 250-350kg of slag deoxidizer are added; (2) Refining and deoxidation white slag making process During the refining and slag-making process, lime, slag-forming agent, slag deoxidizer and aluminum particles are used to make slag; the slag is added in batches, 700-900kg lime, 150-250kg slag-forming agent, 150-250kg slag deoxidizer and 40-60kg aluminum particles are added to the first batch of slag, and 400-600kg lime is added to the second batch of slag 5 minutes after adding, and then the amount of lime is added to 2000kg in batches during the heating process; the argon gas is controlled at 350-450L / min during the heating process; aluminum particles and slag deoxidizer are added according to the actual slag conditions throughout the refining process to maintain white slag, and the aluminum content in the steel is controlled at 0.055%-0.065%, the slag basicity is controlled at 5.5-6.5, and the CaO content in the slag is controlled at 55%-62%; S2. Refining deep desulfurization process On the basis of the previous deoxidation and white slag making, the temperature of molten steel is heated to 1550-1650℃, and deep desulfurization of molten steel is started; the argon gas is adjusted to 750-850L / min of double lines for large argon stirring desulfurization, and the color change of slag is observed during the desulfurization stirring process, and slag deoxidizer is added to maintain the low oxidation of slag; the goal is to reduce the sulfur content in molten steel to 0.0015%; 25-35kg of aluminum particles and 80-120kg of slag deoxidizer are added in the subsequent heating to keep the white slag to avoid heating back oxygen; large argon stirring is strictly prohibited after desulfurization is completed; S3, Refining and Wire Feeding Process In order to reduce the secondary oxidation of molten steel during wire feeding, a soft blowing wire feeding process is adopted; the wire feeding argon gas is set to double-wire 45-55L / min, the wire feeding speed is set to 1.9-2.1m / s, and the feeding calcium wire amount is set to 280-320m; S4, rare earth addition process After wire feeding, soft blowing begins with a double-line argon flow rate of 25-35 L / min. After soft blowing for 2-4 minutes, rare earth alloy is added after the slag liquid surface begins to crust over. After adding the alloy, the soft blowing state is maintained for 3-7 minutes.
2. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: In the above (1): when the steel is tapped to half, 1000 kg of lime and 300 kg of slag deoxidizer are added.
3. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: The first batch of slag material contains 800kg lime, 200kg slag reducing agent, 200kg slag deoxidizer and 50kg aluminum particles.
4. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: 500kg of lime was added to the second batch of slag.
5. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: The argon gas flow rate during the heating process was controlled at 400 L / min.
6. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: Based on the previous deoxidation and white slag making, the molten steel is heated to 1600℃.
7. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: The argon gas was adjusted to a dual-line rate of 800 L / min for large argon stirring desulfurization.
8. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: In S2, 30 kg of aluminum particles and 100 kg of slag deoxidizer are added during subsequent heating to keep the white slag and avoid heating and reoxidation.
9. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: In S3, the wire feeding argon gas is set to double-wire 50 L / min, the wire feeding speed is set to 2 m / s, and the amount of calcium wire fed is set to 300 m.
10. The method for adding rare earth alloy in LF refining furnace according to claim 1, characterized in that: In S4, soft blowing is started after wire feeding, the double-line argon flow rate is 30 L / min, and the rare earth alloy is added after the slag liquid surface begins to crust over for 3 minutes. After the alloy is added, the soft blowing state is maintained for 5 minutes.
Citation Information
Patent Citations
Adding control method for rare earth alloy of rare earth structural steel
CN113416813A
Manufacturing method of rare earth microalloyed weather-resistant bridge steel with yield strength of 370 MPa for high and cold areas
CN113846259A
METHOD FOR TREATING MOLTEN IRON BY ADDITION OF La AND / OR Ce
JP2009024189A
A steel rebar and a production method thereof
US20170029919A1
Cited By
High-rare-earth-content low-carbon steel smelting method for improving nozzle nodulation
CN122081612A