A kind of hard alloy for mining and preparation method thereof

By using WC 75-90%, CoCrFeAlMoN alloy powder, carbonyl nickel coated graphene and ZrO2, combined with atomization nozzle method and SPS sintering technology, mineral cemented carbide with high hardness and strength, solving the traditional solution WC-Co alloys are difficult to meet the problems of high hardness and high strength at the same time, achieving higher flexural strength and microhardness.

CN116287923BActive Publication Date: 2024-11-08CHANGSHA CHAO KING KONG MASCH MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310220510.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-08
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

Traditional WC-Co alloys are difficult to meet the market demands of high hardness and high strength at the same time, especially in the construction of modern mining and infrastructure, the cost and efficiency requirements for cemented carbide are constantly increasing.

Method used

CoCrFeAlMoN alloy powder is prepared by atomizing nozzle method by using mineral cemented carbide composed of WC 75-90%, CoCrFeAlMoN alloy powder 5-10%, carbonyl nickel coated graphene 0.5-1% and ZrO2 1-2%. After stirring in the surfactant solution, zirconium oxychloride and urea reaction is carried out, and then high temperature and high pressure are applied during SPS sintering to form a cemented carbide with high hardness and strength.

Benefits of technology

It improves the hardness and mechanical strength of cemented carbide, refines grains, prevents dislocation movement, enhances flexural strength and microhardness, while reducing structural damage and improving the performance of the bonded phase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116287923B_ABST
    Figure CN116287923B_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal materials, and in particular to a mining cemented carbide and a preparation method thereof. The cemented carbide comprises the following components, by weight: 75-90 parts of WC, 5-10 parts of CoCrFeAlMoN alloy powder, 0.5-1 parts of carbonyl nickel-coated graphene, 1-2 parts of ZrO2, and 1-2 parts of transition metal element carbide. The cemented carbide prepared by the invention has high bending strength and microhardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal materials, in particular to a mining cemented carbide and a preparation method thereof. Background Art

[0002] Cemented carbide is known as the "teeth of industry" and has a history of 90 years since 1923. Over the past 90 years, cemented carbide has been widely used as a high-efficiency tool material and structural material, playing an important role in promoting industrial development and scientific and technological progress.

[0003] As a traditional hard material for mining, WC-Co alloy has the characteristics of strong comprehensive properties such as wear resistance, strength and toughness. In recent years, the vigorous development of mining, energy mining and major infrastructure construction around the world has promoted the widespread application and development of domestic and foreign cemented carbide ball teeth, pick teeth, shield teeth, milling teeth and other mining products. However, with the development of modern science and technology, the end users of the market have higher and higher requirements on the cost and efficiency of cemented carbide. It is difficult for traditional WC-Co alloy to meet the requirements of high hardness and high strength at the same time. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a mining cemented carbide and a preparation method thereof.

[0005] The technical solutions adopted are as follows:

[0006] A mining hard alloy, comprising the following components in parts by weight:

[0007] WC 75-90 parts, CoCrFeAlMoN alloy powder 5-10 parts, carbonyl nickel coated graphene 0.5-1 part, ZrO 2 1-2 parts, transition metal element carbide 1-2 parts.

[0008] Furthermore, the following components are included in parts by weight:

[0009] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, and 2 parts of transition metal element carbide.

[0010] Furthermore, the atomic number ratio of Co, Cr, Fe, Al, Mo and N in the CoCrFeAlMoN alloy powder is 150-200:150-200:70-80:40-60:20-25:1-5, preferably 150:200:75:50:24:1.

[0011] Furthermore, the preparation method of the CoCrFeAlMoN alloy powder is as follows:

[0012] Co, Cr, Fe, Al, and Mo metal powders are heated and melted, and nitrogen gas is introduced to adjust the nitrogen content. The obtained alloy liquid is dropped into an atomizing nozzle and atomized into CoCrFeAlMoN alloy powder under the action of an atomizing medium.

[0013] Furthermore, the atomizing medium is high-purity argon gas, and the atomizing pressure is 4.5-5.5 MPa.

[0014] Furthermore, the preparation method of the carbonyl nickel-coated graphene is as follows:

[0015] The carbonyl nickel is vaporized into steam, and the steam is introduced into a coating furnace to perform vapor deposition coating on the fluidized graphene powder.

[0016] Furthermore, the transition metal carbide is TiC, TaC, VC, Cr 3 C 2 , any one or more combinations of NbC, ZrC, and HfC, wherein the transition metal element carbide is preferably TiC and VC, and the mass ratio of TiC to VC is 1:1.

[0017] The present invention also provides a method for preparing a mining cemented carbide:

[0018] A surfactant solution, a zirconium oxychloride solution and a urea solution are prepared respectively, WC, CoCrFeAlMoN alloy powder, carbonyl nickel-coated graphene and transition metal element carbide are added to the surfactant solution, stirred evenly, and then the zirconium oxychloride solution and the urea solution are added dropwise under heating conditions to react. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed with water and vacuum dried to constant weight, calcined at 550-650° C. for 90-150 minutes under argon protection, and then ball milled. The obtained mixture is loaded into a mold for pre-pressing and then sintered by SPS.

[0019] Furthermore, the pre-pressing pressure is 10-15 MPa and the time is 1-3 min.

[0020] Furthermore, during SPS sintering, the gas pressure in the sintering furnace chamber is pumped down to 6-8 Pa, and sintering is started after applying a pressure of 30-50 MPa, the sintering temperature is 1400-1450° C., and the sintering time is 10-20 min.

[0021] Beneficial effects of the present invention:

[0022] The invention provides a mining cemented carbide, which uses WC as a hard phase, CoCrFeAlMoN alloy powder as a bonding phase, and carbonyl nickel coated with graphene, ZrO 2, transition metal element carbides as reinforcing phases, among which CoCrFeAlMoN alloy powder as a bonding phase has a higher intrinsic hardness than Co bonding phase, which can effectively improve the hardness of cemented carbide. The introduction of N in the bonding phase can improve the wettability of CoCrFeAlMoN alloy powder to WC and improve the mechanical strength. Graphene hinders the growth of grains in the cemented carbide matrix, plays a role in refining grains, and can hinder dislocation movement, thereby improving the strength of cemented carbide. Carbonyl nickel-coated graphene can effectively prevent the dissolution of graphene by alloy elements at high temperatures and reduce the structural damage of graphene. Moreover, compared with nickel coating by electroplating, carbonyl nickel coating has a higher degree of uniformity and introduces fewer impurities, which will not have an adverse effect on the cemented carbide matrix. The in-situ generated ZrO 2 The uniformity of distribution in the cemented carbide is high, which plays a role in solid solution strengthening and grain refinement. The cemented carbide prepared by the present invention has high bending strength and microhardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a metallographic photograph of the mining cemented carbide in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The technologies not mentioned in the present invention are all referenced to the prior art.

[0025] Embodiment 1:

[0026] A mining hard alloy, comprising the following components in parts by weight:

[0027] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, TiC 1 part, VC 1 part;

[0028] The preparation method of the above-mentioned mining cemented carbide is as follows:

[0029] Co with a purity of 99.9wt%, Cr with a purity of 99.9wt%, Fe with a purity of 99.9wt%, Al with a purity of 99.9wt%, and Mo with a purity of 99.9wt% were melted in a pressurized vacuum medium frequency induction furnace. The melting vacuum was 4Pa and the melting temperature was 1650°C. After repeated melting for 5 times, nitrogen was introduced to adjust the nitrogen content. The nitrogen flow rate was 15m 3 / h, the alloy liquid is dropped into the atomizing nozzle, high-purity argon is used as the atomizing medium, the atomizing pressure is 5MPa, and under the action of the atomizing medium, it is atomized into Co 30 Cr 40Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel is introduced into a closed vaporizer for heating and vaporization, the vaporization temperature is 65°C, and the generated carbonyl nickel vapor enters a coating furnace equipped with fluidized graphene powder at a flow rate of 20sccm for vapor deposition coating, the coating furnace temperature is 0-5°C, the graphene powder with carbonyl nickel deposited on the surface is taken out, and a certain volume of 1wt% Span-80 aqueous solution, 5wt% zirconium oxychloride aqueous solution and 5wt% urea aqueous solution (the molar ratio of zirconium oxychloride to urea is 1:1.5) are respectively prepared, and WC, Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel-coated graphene, TiC, and VC were added to Span-80 aqueous solution (solid-liquid mass ratio of 1:10), stirred evenly, heated to 90 °C, and zirconium oxychloride aqueous solution and urea aqueous solution were added dropwise for reaction. After reacting for 5 h, the mixture was cooled to room temperature, filtered, and washed with water until there was no Cl - After that, it was vacuum dried at 80℃ to constant weight, calcined at 600℃ for 120min under argon protection and ball milled for 5h. The obtained mixture was loaded into a graphite mold for pre-pressing. The pre-pressing pressure was 15MPa and the time was 2min. Then it was SPS sintered. During SPS sintering, the air pressure in the sintering furnace chamber was pumped to 8Pa, and sintering began after applying a pressure of 40MPa. The sintering temperature was 1420℃ and the sintering time was 15min.

[0030] Embodiment 2:

[0031] A mining hard alloy, comprising the following components in parts by weight:

[0032] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, TiC 1 part, VC 1 part;

[0033] The preparation method of the above-mentioned mining cemented carbide is as follows:

[0034] Co with a purity of 99.9wt%, Cr with a purity of 99.9wt%, Fe with a purity of 99.9wt%, Al with a purity of 99.9wt%, and Mo with a purity of 99.9wt% were melted in a pressurized vacuum medium frequency induction furnace. The melting vacuum was 4Pa and the melting temperature was 1650°C. After repeated melting for 5 times, nitrogen was introduced to adjust the nitrogen content. The nitrogen flow rate was 15m 3 / h, the alloy liquid is dropped into the atomizing nozzle, high-purity argon is used as the atomizing medium, the atomizing pressure is 5.5MPa, and under the action of the atomizing medium, it is atomized into Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel is introduced into a closed vaporizer for heating and vaporization, the vaporization temperature is 65°C, and the generated carbonyl nickel vapor enters a coating furnace equipped with fluidized graphene powder at a flow rate of 20sccm for vapor deposition coating, the coating furnace temperature is 0-5°C, the graphene powder with carbonyl nickel deposited on the surface is taken out, and a certain volume of 1wt% Span-80 aqueous solution, 5wt% zirconium oxychloride aqueous solution and 5wt% urea aqueous solution (the molar ratio of zirconium oxychloride to urea is 1:1.5) are respectively prepared, and WC, Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel-coated graphene, TiC, and VC were added to Span-80 aqueous solution (solid-liquid mass ratio of 1:10), stirred evenly, heated to 90 °C, and zirconium oxychloride aqueous solution and urea aqueous solution were added dropwise for reaction. After reacting for 5 h, the mixture was cooled to room temperature, filtered, and washed with water until there was no Cl - After that, it was vacuum dried at 80℃ to constant weight, calcined at 650℃ for 150min under argon protection and ball milled for 5h. The obtained mixture was loaded into a graphite mold for pre-pressing. The pre-pressing pressure was 15MPa and the time was 3min. Then it was SPS sintered. During SPS sintering, the air pressure in the sintering furnace chamber was pumped to Pa. After applying a pressure of 50MPa, sintering began. The sintering temperature was 1450℃ and the sintering time was 20min.

[0035] Embodiment 3:

[0036] A mining hard alloy, comprising the following components in parts by weight:

[0037] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, TiC 1 part, VC 1 part;

[0038] The preparation method of the above-mentioned mining cemented carbide is as follows:

[0039] Co with a purity of 99.9wt%, Cr with a purity of 99.9wt%, Fe with a purity of 99.9wt%, Al with a purity of 99.9wt%, and Mo with a purity of 99.9wt% were melted in a pressurized vacuum medium frequency induction furnace. The melting vacuum was 4Pa and the melting temperature was 1650°C. After repeated melting for 5 times, nitrogen was introduced to adjust the nitrogen content. The nitrogen flow rate was 15m 3 / h, the alloy liquid is dropped into the atomizing nozzle, high-purity argon is used as the atomizing medium, the atomizing pressure is 4.5MPa, and under the action of the atomizing medium, it is atomized into Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel is introduced into a closed vaporizer for heating and vaporization, the vaporization temperature is 65°C, and the generated carbonyl nickel vapor enters a coating furnace equipped with fluidized graphene powder at a flow rate of 20sccm for vapor deposition coating, the coating furnace temperature is 0-5°C, the graphene powder with carbonyl nickel deposited on the surface is taken out, and a certain volume of 1wt% Span-80 aqueous solution, 5wt% zirconium oxychloride aqueous solution and 5wt% urea aqueous solution (the molar ratio of zirconium oxychloride to urea is 1:1.5) are respectively prepared, and WC, Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel-coated graphene, TiC, and VC were added to Span-80 aqueous solution (solid-liquid mass ratio of 1:10), stirred evenly, heated to 90 °C, and zirconium oxychloride aqueous solution and urea aqueous solution were added dropwise for reaction. After reacting for 5 h, the mixture was cooled to room temperature, filtered, and washed with water until there was no Cl - After that, it was vacuum dried at 80℃ to constant weight, calcined at 550℃ for 90min under argon protection and ball milled for 5h. The obtained mixture was loaded into a graphite mold for pre-pressing. The pre-pressing pressure was 10MPa and the time was 1min. Then it was SPS sintered. During SPS sintering, the air pressure in the sintering furnace chamber was pumped to 6Pa, and sintering began after applying a pressure of 30MPa. The sintering temperature was 1400℃ and the sintering time was 10min.

[0040] Embodiment 4:

[0041] A mining hard alloy, comprising the following components in parts by weight:

[0042] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, TiC 1 part, VC 1 part;

[0043] The preparation method of the above-mentioned mining cemented carbide is as follows:

[0044] Co with a purity of 99.9wt%, Cr with a purity of 99.9wt%, Fe with a purity of 99.9wt%, Al with a purity of 99.9wt%, and Mo with a purity of 99.9wt% were melted in a pressurized vacuum medium frequency induction furnace. The melting vacuum was 4Pa and the melting temperature was 1650°C. After repeated melting for 5 times, nitrogen was introduced to adjust the nitrogen content. The nitrogen flow rate was 15m 3 / h, the alloy liquid is dropped into the atomizing nozzle, high-purity argon is used as the atomizing medium, the atomizing pressure is 5.5MPa, and under the action of the atomizing medium, it is atomized into Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel is introduced into a closed vaporizer for heating and vaporization, the vaporization temperature is 65°C, and the generated carbonyl nickel vapor enters a coating furnace equipped with fluidized graphene powder at a flow rate of 20sccm for vapor deposition coating, the coating furnace temperature is 0-5°C, the graphene powder with carbonyl nickel deposited on the surface is taken out, and a certain volume of 1wt% Span-80 aqueous solution, 5wt% zirconium oxychloride aqueous solution and 5wt% urea aqueous solution (the molar ratio of zirconium oxychloride to urea is 1:1.5) are respectively prepared, and WC, Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel-coated graphene, TiC, and VC were added to Span-80 aqueous solution (solid-liquid mass ratio of 1:10), stirred evenly, heated to 90 °C, and zirconium oxychloride aqueous solution and urea aqueous solution were added dropwise for reaction. After reacting for 5 h, the mixture was cooled to room temperature, filtered, and washed with water until there was no Cl - After that, it was vacuum dried at 80℃ to constant weight, calcined at 550℃ for 150min under argon protection and ball milled for 5h. The obtained mixture was loaded into a graphite mold for pre-pressing. The pre-pressing pressure was 10MPa and the time was 3min. Then it was SPS sintered. During SPS sintering, the air pressure in the sintering furnace chamber was pumped to 6Pa, and sintering began after applying a pressure of 50MPa. The sintering temperature was 1400℃ and the sintering time was 20min.

[0045] Embodiment 5:

[0046] A mining hard alloy, comprising the following components in parts by weight:

[0047] WC 88 parts, CoCrFeAlMoN alloy powder 6 parts, carbonyl nickel coated graphene 0.5 parts, ZrO 2 1.5 parts, TiC 1 part, VC 1 part;

[0048] The preparation method of the above-mentioned mining cemented carbide is as follows:

[0049] Co with a purity of 99.9wt%, Cr with a purity of 99.9wt%, Fe with a purity of 99.9wt%, Al with a purity of 99.9wt%, and Mo with a purity of 99.9wt% were melted in a pressurized vacuum medium frequency induction furnace. The melting vacuum was 4Pa and the melting temperature was 1650°C. After repeated melting for 5 times, nitrogen was introduced to adjust the nitrogen content. The nitrogen flow rate was 15m 3 / h, the alloy liquid is dropped into the atomizing nozzle, high-purity argon is used as the atomizing medium, the atomizing pressure is 4.5MPa, and under the action of the atomizing medium, it is atomized into Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 alloy powder, introduce carbonyl nickel into a closed vaporizer for heating and vaporization, the vaporization temperature is 65°C, and the generated carbonyl nickel vapor enters a coating furnace equipped with fluidized graphene powder at a flow rate of 20sccm for vapor deposition coating, the coating furnace temperature is 0-5°C, the graphene powder with carbonyl nickel deposited on the surface is taken out, and a certain volume of 1wt% Span-80 aqueous solution, 5wt% zirconium oxychloride aqueous solution and 5wt% urea aqueous solution (the molar ratio of zirconium oxychloride to urea is 1:1.5) are respectively prepared, and WC, Co 30 Cr 40 Fe 15 Al 10 Mo 4.8 N 0.2 Alloy powder, carbonyl nickel-coated graphene, TiC, and VC were added to Span-80 aqueous solution (solid-liquid mass ratio of 1:10), stirred evenly, heated to 90 °C, and zirconium oxychloride aqueous solution and urea aqueous solution were added dropwise for reaction. After reacting for 5 h, the mixture was cooled to room temperature, filtered, and washed with water until there was no Cl - After that, it was vacuum dried at 80℃ to constant weight, calcined at 650℃ for 90min under argon protection and ball milled for 5h. The obtained mixture was loaded into a graphite mold for pre-pressing. The pre-pressing pressure was 15MPa and the time was 1min. Then it was SPS sintered. During SPS sintering, the air pressure in the sintering furnace chamber was pumped to 8Pa, and sintering began after applying a pressure of 30MPa. The sintering temperature was 1450℃ and the sintering time was 10min.

[0050] Comparative Example 1:

[0051] Basically the same as Example 1, except that the graphene is not coated with carbonyl nickel.

[0052] Comparative Example 2:

[0053] It is basically the same as Example 1, except that the same mass of nickel is directly added as a raw material.

[0054] Comparative Example 3:

[0055] The method is basically the same as Example 1, except that the CoCrFeAlMo alloy powder of the same mass is used to replace the CoCrFeAlMoN alloy powder, and the atomic ratios of Co, Cr, Fe, Al and Mo are the same.

[0056] Performance Test:

[0057] The hard alloys prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention were used as samples for performance testing. The prepared samples were processed by electric spark wire cutting, the surface was ground with a diamond grinding wheel, and the ground samples were polished. The bending strength and transverse rupture strength of the hard alloy were tested according to GB / T3851-2015, and the microhardness of the hard alloy was tested according to GB / T7997-2014. The test results are shown in Table 1 below:

[0058] Table 1:

[0059]

[0060] It can be seen from Table 1 above that the cemented carbide prepared by the present invention has higher bending strength and microhardness.

[0061] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A cemented carbide for mining, characterized in that: The raw materials used are composed of the following components by weight: WC 75-90 parts, CoCrFeAlMoN alloy powder 5-10 parts, carbonyl nickel coated graphene 0.5-1 part, zirconium oxychloride and urea with 1-2 parts of ZrO2 generated in situ, and transition metal element carbide 1-2 parts; The atomic number ratio of Co, Cr, Fe, Al, Mo and N in the CoCrFeAlMoN alloy powder is 150-200: 150-200: 70-80: 40-60: 20-25: 1-5.

2. The mining cemented carbide according to claim 1, characterized in that: The raw materials used are composed of the following components by weight: 88 parts of WC, 6 parts of CoCrFeAlMoN alloy powder, 0.5 parts of carbonyl nickel-coated graphene, 1.5 parts of zirconium oxychloride and urea generated in situ of ZrO2, and 2 parts of transition metal element carbide.

3. The mining cemented carbide according to claim 1, characterized in that: The atomic number ratio of Co, Cr, Fe, Al, Mo and N in the CoCrFeAlMoN alloy powder is 150:200:75:50:24:

1.

4. The mining cemented carbide according to claim 1, characterized in that: The preparation method of the CoCrFeAlMoN alloy powder is as follows: Co, Cr, Fe, Al, and Mo metal powders are heated and melted, and nitrogen gas is introduced to adjust the nitrogen content. The obtained alloy liquid is dropped into an atomizing nozzle and atomized into CoCrFeAlMoN alloy powder under the action of an atomizing medium.

5. The mining cemented carbide according to claim 4, characterized in that: The atomizing medium is high-purity argon gas, and the atomizing pressure is 4.5-5.5 MPa.

6. The mining cemented carbide according to claim 1, characterized in that: The preparation method of the carbonyl nickel-coated graphene is as follows: The carbonyl nickel is vaporized into steam, and the steam is introduced into a coating furnace to perform vapor deposition coating on the fluidized graphene powder.

7. The mining cemented carbide according to claim 1, characterized in that: The transition metal element carbide is any one of TiC, TaC, VC, Cr3C2, NbC, ZrC, and HfC, or a combination of two or more thereof.

8. A method for preparing a mining cemented carbide as claimed in any one of claims 1 to 7, characterized in that: A surfactant solution, a zirconium oxychloride solution and a urea solution are prepared respectively, WC, CoCrFeAlMoN alloy powder, carbonyl nickel-coated graphene and transition metal element carbide are added to the surfactant solution, stirred evenly, and then the zirconium oxychloride solution and the urea solution are added dropwise under heating conditions to react. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed with water and vacuum dried to constant weight, calcined at 550-650° C. for 90-150 minutes under argon protection, and then ball milled. The obtained mixture is loaded into a mold for pre-pressing and then sintered by SPS.

9. The method for preparing a mining cemented carbide according to claim 8, characterized in that: The pre-pressing pressure is 10-15MPa and the time is 1-3min.

10. The method for preparing a mining cemented carbide according to claim 8, characterized in that: During SPS sintering, the gas pressure in the sintering furnace chamber is pumped to 6-8Pa, and sintering begins after applying a pressure of 30-50MPa. The sintering temperature is 1400-1450℃, and the sintering time is 10-20min.