A method for producing a single-batch multi-stage pipeline steel plate

Through a pipeline steel chemical composition system and specific process flow, including heating, coiling, fly shears and ultra-fast cooling, the problem of difficult production of multi-stage pipeline steel is solved, and efficient production of pipeline steel plates of different levels is achieved. and excellent low temperature toughness performance.

CN116288036BActive Publication Date: 2024-11-29SD STEEL RIZHAO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211101216.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-11-29
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

Multi-stage pipeline steel cannot be produced in the steelmaking process, and continuous casting process cannot be continuously cast, resulting in high difficulty in the production of steel plates, with more residual blanks and residual materials, and high operating costs.

Method used

A pipeline steel chemical composition system is adopted to realize the production of pipeline steel plates of different levels through heating, coiling, fly shears and ultra-fast cooling processes. This method includes casting billet heating, coil rolling, fly shear segmentation and ultra-fast cooling of high-pressure segments to ensure stable performance of steel plates of different levels.

Benefits of technology

The production of pipeline steel products of different strength levels has been achieved. The steel plate has excellent low-temperature toughness, which reduces the production organization difficulty, the number of residual blanks and residual materials, reduces the operating costs, and meets the needs of various users.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288036B_ABST
    Figure CN116288036B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of pipeline steel production, and specifically to a method for producing a one-bill multi-grade pipeline steel plate, comprising heating the ingot, rolling, flying shearing, and ultra-rapid cooling; wherein the multi-grade pipeline steel plates are X52, X56, X60, and X65 grade pipeline steel plates. The present invention can realize the one-bill production of pipeline steel products of different strength levels, and the steel plates obtained have excellent low-temperature toughness. The present invention reduces the difficulty of organizing the production of large orders of pipeline steel, reduces the number of surplus billets and surplus materials, and reduces operating costs; the billet assembly is more flexible, which is conducive to ensuring stable performance and meeting the needs of various users.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipeline steel production, and in particular to a method for producing a single-batch multi-stage pipeline steel plate. Background Art

[0002] Pipeline transportation is listed as one of the five major modern transportation modes along with railway transportation, road transportation, water transportation and air transportation; pipeline steel is a carrier for transporting energy such as oil and natural gas. With the development of pipeline engineering, the technical requirements for the strength and toughness of pipeline steel are increasing. Due to the differences in service areas and uses of pipeline steel, pipeline steel is also a special type of steel that can meet the needs of different customers, and needs to be designed and produced with separate chemical composition according to customer needs. The difference in chemical composition inevitably causes problems such as the inability to produce multi-level pipeline steel in the steelmaking process and the inability to continuously cast in the continuous casting process, which is not conducive to the production organization of steel plates. Therefore, designing a reasonable and low-cost chemical composition system suitable for the production of multi-level pipeline steel, and through reasonable and precise process design, using a pipeline steel chemical composition system to produce different levels of pipeline steel plates can reduce the difficulty of organizing the production of large orders of pipeline steel, reduce the number of residual billets and residual materials, and reduce operating costs. The billet assembly is more flexible, which is conducive to ensuring stable performance and meeting the needs of various users. Summary of the invention

[0003] In view of the technical problem that multi-grade pipeline steels cannot be produced simultaneously, the present invention provides a method for producing a single-batch multi-grade pipeline steel plate, which can realize the single-batch production of pipeline steel products of different strength levels, and the produced steel plates all have excellent low-temperature toughness performance.

[0004] The present invention provides a method for producing a single-bill multi-grade pipeline steel plate, comprising heating the ingot, rolling, flying shearing and ultra-rapid cooling; wherein the multi-grade pipeline steel plate is respectively X52, X56, X60 and X65 grade pipeline steel plates.

[0005] Furthermore, the pipeline steel plate includes the following chemical components in weight percentage: C 0.06%~0.09%, Si 0.20%~0.35%, Mn 1.45%~1.60%, P≤0.012%, S≤0.003%, Nb 0.030%~0.050%, Ti 0.008%~0.020%, Als 0.020%~0.050%, and the rest are Fe and residual elements; the ingot thickness is 150 mm.

[0006] Furthermore, the heating process of the ingot is as follows: when the thickness of the finished steel is h, the furnace temperature is 1200-1240°C when h<8mm; when h≥8mm, the furnace temperature is 1170-1210°C; and the heating time is 8-13min / cm.

[0007] Furthermore, the coil rolling is carried out by a 3500 mm Steckel mill, with a total of 11 rolling passes; the thickness of the finished steel is h;

[0008] When h<8mm, 6+5 passes are used for rolling, of which 6 is the rough rolling pass, 5 is the coiling and finishing pass, the final rolling temperature is 850℃, the coiling furnace temperature is 950℃, the rolling mode is non-temperature controlled coiling, and the final rolling speed is 1.8m / s;

[0009] When 8mm≤h<12mm, the intermediate billet thickness is 45-50mm, and 5+3+3 passes are adopted, wherein 5 is the rough rolling pass, 3+3 are the finishing passes of flat rolling and coiling respectively, the final rolling temperature is 840-860℃, the coiling furnace temperature is 900-940℃, the rolling mode is temperature-controlled coiling, and the final rolling speed is 1.6-1.8m / s;

[0010] When 12mm≤h<16mm, the intermediate billet thickness is 55-60mm, and 5+3+3 passes are adopted, wherein 5 is the rough rolling pass, 3+3 are the finishing passes of flat rolling and coiling respectively, the final rolling temperature is 820-840℃, the coiling furnace temperature is 860-900℃, the rolling mode is temperature-controlled coiling, and the final rolling speed is 1.4-1.6m / s.

[0011] Furthermore, the flying shear process is that according to the length of the finished steel plate, the flying shear divides the entire mother plate into several sections, and the steel plates of the same level are divided into the same section, and the section length is ≤50m; each section of the steel plate is allocated from the beginning to the end of the mother plate in the order from low-level to high-level steel plates.

[0012] Furthermore, after the steel plates are segmented by level, the front and rear sections of the steel plates are pulled 1m apart through roller micro-acceleration control to ensure that the ultra-fast cooling actuator has sufficient time to adjust the water volume difference between the front and rear plates.

[0013] Furthermore, the ultra-fast cooling process is to use ultra-fast cooling in the high-pressure section + conventional accelerated cooling in the low-pressure section; the ultra-fast cooling in the high-pressure section has a cooling rate of 30-60°C / s, and the water pressure is 0.2-0.5MPa; the conventional accelerated cooling in the low-pressure section has a cooling rate of 10-30°C / s, and the water pressure is 0.2MPa. Furthermore, in the ultra-fast cooling process, the final cooling temperatures of X52, X56, X60, and X65 grade pipeline steel plates are 650±20°C, 620±20°C, 580±20°C, and 540±20°C, respectively.

[0014] Furthermore, in the ultra-fast cooling process, the temperature fed back to the model by the ultra-fast cooling inlet pyrometer is calculated. The model is a self-learning model, which can automatically set the number of high-pressure or low-pressure sections and the amount of water to be opened according to the previous cooling rate, plate type and other parameters. In addition, the ultra-fast cooling tracking system can track the head and tail positions of each segmented plate. It ensures that the same slab produces different grades of pipeline steel with stable performance, and there will be no unstable performance areas in the entire mother plate due to the adjustment of water volume or water group number.

[0015] The control method of the amount of water and number of groups required for each section of steel plate is:

[0016] The ultra-fast cooling detection elements are arranged as follows: the Tb pyrometer is located at the mill exit for pre-calculated temperature detection; the T1 pyrometer is located before the flying shear for corrected calculated temperature detection; the T2 pyrometer is located before ultra-fast cooling for start-cooling temperature detection;

[0017] The water volume basic flow rate is set to 75m in the database 3 / h, and set the upper limit flow rate ≤150m 3 / h;

[0018] In the coil rolling water cooling model, the water cooling correction calculation adopts the mode of pre-calculated flow multiplied by correction coefficient and fixed number of groups;

[0019] When the head of the mother plate passes through the Tb pyrometer, the Tb pyrometer feeds back the detected temperature to the model to trigger pre-calculation, and obtains the pre-calculated water volume and number of groups of the steel plate; when the head of the mother plate passes through the T1 pyrometer, the first stage of steel plate correction calculation is performed to fix the number of groups and flow rate;

[0020] When the mother plate is divided into sections by flying shear, the head of each section of the steel plate passes through the T1 pyrometer, and the T1 pyrometer feeds the detected temperature back to the model for correction calculation to obtain the corrected water volume of each section of the steel plate;

[0021] The first-level tracking system tracks the head and tail positions of each segment, and the actuator adjusts the water volume group by group before the head reaches the header based on the head and tail tracking positions.

[0022] The beneficial effects of the present invention are:

[0023] (1) The present invention can use one slab and one component system to produce four different grades of pipeline steel plates, with the steel plate specifications ranging from 6 to 16 mm in thickness and the mother plate length ranging from 100 to 400 m, thereby solving the problem that multiple grades of pipeline steel cannot be produced in one furnace in the steelmaking process and cannot be continuously cast in the continuous casting process;

[0024] (2) The present invention adopts a low-carbon component design, adds appropriate amounts of Nb and Ti alloys for microalloying, eliminates the Cr element, combines appropriate controlled rolling and controlled cooling process control, increases the cooling rate through an ultra-fast cooling and high-pressure section, and gives full play to the effects of fine grain strengthening, precipitation strengthening and phase transformation strengthening, thereby achieving the production of pipeline steel products of different strength levels and having excellent low-temperature toughness properties;

[0025] (3) The present invention adopts the flying shear segmentation and roller micro-acceleration and water cooling process to ensure the stable performance of pipeline steel of different grades produced from the same slab;

[0026] (4) The present invention reduces the difficulty of organizing the production of large orders of pipeline steel, reduces the number of surplus billets and surplus materials, and reduces operating costs; the billet assembly is more flexible, which is conducive to ensuring stable performance and meeting the needs of various users. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0028] Figure 1 It is a layout diagram of ultrafast cooling detection elements according to a specific embodiment of the present invention.

[0029] Figure 2 This is a diagram of the interface for setting the ultrafast cooling water cooling correction calculation mode according to a specific implementation mode of the present invention.

[0030] Figure 3 It is a metallographic structure diagram of X52 pipeline steel plate obtained according to a specific implementation method of the present invention.

[0031] Figure 4 It is a metallographic structure diagram of X56 pipeline steel plate obtained according to a specific implementation method of the present invention.

[0032] Figure 5 It is a metallographic structure diagram of X60 pipeline steel plate obtained according to a specific implementation method of the present invention.

[0033] Figure 6 It is a metallographic structure diagram of X65 pipeline steel plate obtained according to a specific implementation method of the present invention. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0035] Example 1

[0036] The present invention adopts one slab and one component system to produce four different grades of pipeline steel plates.

[0037] Example 1 Select rolling 10mm×2580mm×200m X52, X56, X60, X65 actual order pipeline steel plates, the production process includes the following steps:

[0038] (1) Heating

[0039] A 150 mm thick continuous casting billet is used, and its chemical composition (by weight percentage) is as follows: C 0.07%, Si 0.30%, Mn 1.50%, P≤0.012%, S≤0.003%, Nb 0.040%, Ti 0.010%, Als 0.030%, and the rest are Fe and residual elements; the continuous casting billet is heated out of the furnace at a temperature of 1200°C, and the heating time is controlled at 9 min / cm;

[0040] (2) Coil rolling

[0041] The steel was rolled by a Steckel mill with 5+3+3 passes, and the intermediate billet thickness was set to 45 mm. The final rolling temperature was set to 850°C, the coiling furnace temperature was set to 920°C, the rolling mode was temperature-controlled rolling, and the final rolling speed was set to 1.8 m / s.

[0042] (3) Flying shear

[0043] The 200m long mother plate flying shear is divided into 4 sections, and the steel plates of the same grade are divided into the same section, each section is 50m, and each section of steel plates is distributed from low grade to high grade along the mother plate from the beginning to the end. The grades of the 4 sections of steel plates are X52, X56, X60, and X65 grade pipeline steel plates. After the steel plates are divided into sections according to grades, the front and rear sections of the steel plates are pulled apart by 1m through micro-acceleration control;

[0044] (4) Ultra-fast cooling

[0045] Ultra-fast cooling adopts ultra-fast cooling in high-pressure section + conventional accelerated cooling in low-pressure section. The final cooling temperature is set for the four sections of steel plates divided by the flying shear, and is set to 650℃, 620℃, 580℃ and 540℃ from the beginning to the end;

[0046] The high-pressure section ultra-fast cooling mode is turned on, the water pressure is set to 0.3MPa, and the rapid cooling rate is 50℃ / s; the cooling type is set to give priority to the high-pressure section, and the conventional accelerated cooling rate of the low-pressure section is 20℃ / s, and the water pressure is 0.2MPa. Before each section of steel plate enters the ultra-fast cooling, the pyrometer at the ultra-fast cooling entrance detects the opening temperature of the cooling, and the pyrometer feeds the temperature back to the model. Figure 1 The arrangement of ultrafast cooling detection elements is shown. The Tb pyrometer is located at the mill exit for pre-calculated temperature detection; the T1 pyrometer is located before the flying shear for corrected calculated temperature detection; the T2 pyrometer is located before ultrafast cooling for start-cooling temperature detection.

[0047] In the rolling water cooling model, the water cooling correction calculation is the flow rate multiplied by the correction coefficient (such as Figure 2 As shown in the figure, the mode of fixing the number of groups and adjusting the flow rate is used. The water volume and number of groups required for each section of steel plate are calculated by modifying the model according to the final cooling temperature. The basic water flow rate is set to 75m in the database. 3 / h, and set the upper limit flow rate ≤150m 3 / h;

[0048] Combination Figure 1 , the control method is as follows:

[0049] The Tb pyrometer sends the head temperature of the rolled steel plate to the ultra-fast cooling model for pre-calculation of the number of groups and flow rate. The 75m 3 / h, open 13 sets of headers; the head of the steel plate passes through the T1 pyrometer, and the T1 pyrometer feeds back the detected temperature to the model for correction calculation, and calculates the number of groups and flow rate used by the first section of steel plate, which are 75m 3 / h and 10 sets of headers, and sent to the first level for execution; when the flying shear performs the first shearing, the T1 pyrometer sends the detected temperature of the second section of the steel plate to the model, and the flow rate of the second section is corrected and calculated according to the final cooling temperature, and the flow rate is set to 80m 3 / h, and sent it to the first level. The actuator changes the flow rate from 75m / h to 3 / h increases to 80m per group 3 / h, the third and fourth sections are calculated in sequence according to the above rules; the distance between the front plate and the rear plate of each section of steel plate is 1m, and the first-level tracking system tracks the head and tail positions of each section. Therefore, the actuator adjusts the water volume group by group according to the head and tail tracking positions before the head reaches the header.

[0050] The physical properties of each section of 10 mm thick 4 different grades of pipeline steel were tested by sampling at the head, middle and tail. The specific results are shown in Table 1.

[0051] Table 1 Specific data of physical properties test of pipeline steel plates of different grades obtained in Example 1

[0052]

[0053]

[0054] Figure 3 , Figure 4 , Figure 5 and Figure 6 The metallographic structures of the four different grades of pipeline steel plates are shown respectively, and their specific metallographic structures and corresponding physical property data are shown in Table 2.

[0055] Table 1 Metallographic structures and corresponding physical properties of 4 different grades of pipeline steel plates obtained in Example 1

[0056]

[0057] It can be seen from Tables 1 and 2 that the performance indicators of the four grades of steel plate products meet the GB / T14164-2103 standards, and the drop hammer performance meets the low-temperature crack arrest toughness requirement of 0--30℃ drop hammer shear area ≥85%.

[0058] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A method for producing a single-batch multi-stage pipeline steel plate, characterized in that: It includes heating, rolling, flying shearing and ultra-fast cooling of the ingot; the multi-grade pipeline steel plates are X52, X56, X60 and X65 grade pipeline steel plates; The pipeline steel plate includes the following chemical compositions in weight percentage: C 0.06%~0.09%, Si 0.20%~0.35%, Mn1.45%~1.60%, P≤0.012%, S≤0.003%, Nb 0.030%~0.050%, Ti 0.008%~0.020%, Als 0.020%~0.050%, and the rest are Fe and residual elements; the ingot thickness is 150mm; The flying shear process is to divide the whole mother plate into several sections according to the length of the finished steel plate, and divide the steel plates of the same grade into the same section, with the length of the section ≤ 50m; each section of steel plate is distributed from the beginning to the end of the mother plate in the order from low grade to high grade steel plates; After the steel plates are divided into sections according to their levels, the front and rear sections of the steel plates are pulled 1m apart through micro-acceleration control; In the ultra-fast cooling process, the water volume and group number control method for each section of steel plate is as follows: The water volume basic flow rate is set to 75m in the database 3 / h, and set the upper limit flow rate ≤150m 3 / h; In the coil rolling water cooling model, the water cooling correction calculation adopts the mode of pre-calculated flow multiplied by correction coefficient and fixed number of groups; When the head of the mother steel plate passes through the Tb pyrometer, the Tb pyrometer feeds back the detected temperature to the model to trigger pre-calculation, and obtains the pre-calculated water volume and group number of the steel plate; When the head of the mother plate passes through the T1 high temperature timer, the first section of the plate correction calculation is performed to fix the number of groups and flow rate; When the mother plate is divided into sections by flying shear, the head of each section of the steel plate passes through the T1 pyrometer, and the T1 pyrometer feeds the detected temperature back to the model for correction calculation to obtain the corrected water volume of each section of the steel plate; The first-level tracking system tracks the head and tail positions of each segment, and the actuator adjusts the water volume group by group before the head reaches the header according to the head and tail tracking positions; The ultra-fast cooling process is to use ultra-fast cooling in the high-pressure section + conventional accelerated cooling in the low-pressure section; The ultra-fast cooling rate of the high-pressure section is 30~60℃ / s, and the water pressure is 0.2~0.5MPa; the conventional accelerated cooling rate of the low-pressure section can reach 10~30℃ / s, and the water pressure is 0.2MPa; In the ultra-fast cooling process, the final cooling temperatures of X52, X56, X60 and X65 grade pipeline steel plates are 650±20℃, 620±20℃, 580±20℃ and 540±20℃ respectively.

2. The method for producing a single-batch multi-stage pipeline steel plate according to claim 1, characterized in that: The heating process of the ingot is as follows: the thickness of the finished steel is h, when h<8mm, the furnace temperature is 1200~1240℃; when h≥8mm, the furnace temperature is 1170~1210℃; the heating time is 8~13min / cm.

3. The method for producing a single-batch multi-stage pipeline steel plate according to claim 1, characterized in that: The coil is rolled using a Steckel mill, with a total of 11 passes; the thickness of the finished steel is h; When h<8mm, the final rolling temperature is 850℃, the coiling furnace temperature is 950℃, the rolling mode is non-temperature controlled coiling, and the final rolling speed is 1.8m / s; When 8mm≤h<12mm, the intermediate billet thickness is 45~50mm, the final rolling temperature is 840~860℃, the coiling furnace temperature is 900~940℃, the rolling mode is temperature-controlled coiling, and the final rolling speed is 1.6~1.8m / s; When 12mm≤h<16mm, the intermediate billet thickness is 55~60mm, the final rolling temperature is 820~840℃, the coiling furnace temperature is 860~900℃, the rolling mode is temperature-controlled coiling, and the final rolling speed is 1.4~1.6m / s.

Citation Information

Patent Citations

  • Method for producing X65 acid-resistant pipeline steel plate used under low-cost and ultralow-temperature conditions through curling furnace

    CN112410647A

  • Production method of one-steel multi-stage high-toughness pipeline steel hot-rolled coil plate

    CN114657442A