Solar cell manufacturing method

By forming doped emitter layers on the front and back of the silicon wafer and performing laser bombardment, the problems of insufficient conductivity and surface heating in the existing technology are solved, and the electrical performance of the solar cell is significantly improved.

CN116314462BActive Publication Date: 2024-10-01TRINA SOLAR (YANCHENG TINGHU) OPTOELECTRONICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310300852.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-01
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Existing crystalline silicon solar cells have poor electrical performance, especially insufficient conductivity and surface heating problems during the design and manufacturing process of the passivation layer and emitter layer, which affect the overall performance of the solar cell.

Method used

Doped emitter layers and passivation layers are formed on the front and back sides of the silicon wafer respectively, and laser bombardment is performed before or after the formation of these layers to activate doping. The laser bombardment method is used to replace the traditional high-temperature diffusion technology to improve conductivity. and open circuit voltage.

Benefits of technology

Activating doping by laser bombardment reduces the saturation current density and surface heating of the emitter, improves the conductivity and implicit open circuit voltage of the solar cell, and significantly improves the electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116314462B_ABST
    Figure CN116314462B_ABST
Patent Text Reader

Abstract

In the embodiment of the present disclosure, a method for manufacturing a solar cell is provided, wherein a doped emitter layer is formed on the front side of a silicon wafer, a first passivation layer is formed on the emitter layer, and a second passivation layer is formed on the back side of the silicon wafer, and before or after the first passivation layer and the second passivation layer are formed, the emitter layer is laser-bombarded to activate the doping. Compared with the high-temperature diffusion technology used in the related art, the embodiment of the present disclosure proposes to use a laser-bombardment method to activate the doping of the emitter layer, which reduces the emitter saturation current density and surface heating, while providing enhanced conductivity and implicit open-circuit voltage, thereby improving the electrical performance of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of photovoltaic technology, and in particular to a method for manufacturing a solar cell. Background Art

[0002] In the field of crystalline silicon solar cell technology, tunneling oxide passivating contacts (TOPCon) technology is an excellent cell passivation technology.

[0003] The passivation layer in the TOPCon battery structure can inhibit carrier recombination on the surface of the silicon wafer, improve the minority carrier lifetime of the silicon wafer and the open circuit voltage of the battery. The carrier selective collection passivation contact structure can be applied to the entire surface of the battery without the need to open holes to form local passivation contacts. This not only simplifies the manufacturing process, but also the carriers only need to be transported in one-dimensional direction without the need for additional lateral transmission, thereby achieving a higher fill factor. Summary of the invention

[0004] In view of the above shortcomings of the related art, the purpose of the present disclosure is to provide a method for manufacturing a solar cell to solve the technical problem of poor electrical performance of the related art solar cell.

[0005] A first aspect of the present disclosure provides a method for manufacturing a solar cell, comprising:

[0006] forming a doped emitter layer on the front side of the silicon wafer;

[0007] forming a first passivation layer on the emitter layer and a second passivation layer on the back side of the silicon wafer;

[0008] Before or after forming the first passivation layer and the second passivation layer, the emitter layer is laser-bombarded to activate doping.

[0009] Optionally, forming a doped emitter layer on the front side of the silicon wafer includes:

[0010] The emitter layer is deposited on the front side of the silicon wafer using PH3, O2 and SiH4 as precursors.

[0011] Optionally, forming a doped emitter layer on the front side of the silicon wafer includes:

[0012] The emitter is deposited on the front side of the silicon wafer using BN2 and BCI3 as precursors.

[0013] Optionally, the laser irradiation energy range during the laser bombardment process is: 0.3-0.4 J / cm 2 .

[0014] Optionally, the laser pulse overlap rate during the laser bombardment process is 40%-60%.

[0015] Optionally, the laser irradiation energy range during the laser bombardment process is: 0.38 J / cm 2 .

[0016] Optionally, the solar cell manufacturing method further comprises:

[0017] Before forming a doped emitter layer on the front side of the silicon wafer, a first silicon oxide layer is deposited on the front side of the silicon wafer, and the emitter layer covers the first silicon oxide layer.

[0018] Optionally, the solar cell manufacturing method further comprises:

[0019] Before forming the second passivation layer on the back side of the silicon wafer, a passivation contact layer is deposited on the back side of the silicon wafer, and the second passivation layer is located on the side of the passivation contact layer facing away from the silicon wafer.

[0020] Optionally, a passivation contact layer is deposited on the back side of the silicon wafer, comprising:

[0021] Depositing a second silicon oxide layer on the back side of the silicon wafer;

[0022] Using SiH4, O2 and B2H6 as precursors, amorphous silicon is deposited on the side of the second silicon oxide layer facing away from the silicon wafer. The amorphous silicon is crystallized during laser bombardment to be converted into a polycrystalline silicon layer. The second silicon oxide layer and the polycrystalline silicon layer constitute a passivation contact layer.

[0023] Optionally, forming a first passivation layer on the emitter layer and forming a second passivation layer on the back side of the silicon wafer comprises:

[0024] A first passivation layer is formed on the emitter layer and a second passivation layer is formed on the back side of the silicon wafer by using a plasma enhanced chemical vapor deposition method, and high temperature annealing is performed.

[0025] As described above, the disclosed embodiment provides a method for manufacturing a solar cell, by forming a doped emitter layer on the front side of a silicon wafer, forming a first passivation layer on the emitter layer and forming a second passivation layer on the back side of the silicon wafer, and before or after forming the first passivation layer and the second passivation layer, laser bombarding the emitter layer to activate doping. Using this embodiment, compared with the high-temperature diffusion technology used in the related art, the disclosed embodiment proposes to use a laser bombardment method to activate the doping of the emitter layer, while reducing the emitter saturation current density and surface heating, providing enhanced conductivity and implicit open circuit voltage, thereby improving the electrical performance of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A flow chart showing a method for manufacturing a solar cell according to an embodiment of the present disclosure.

[0027] Figure 2-4 A schematic diagram showing the product structure of each stage of a solar cell manufacturing method according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0028] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the information disclosed in the present disclosure. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in the present disclosure can also be modified or changed in various ways according to different viewpoints and application systems without departing from the spirit of the present disclosure. It should be noted that the embodiments and features in the embodiments in the present disclosure can be combined with each other without conflict.

[0029] The following is a detailed description of the embodiments of the present disclosure with reference to the accompanying drawings so that those skilled in the art can easily implement the present disclosure. The present disclosure can be embodied in many different forms and is not limited to the embodiments described herein.

[0030] In the representations of the present disclosure, the reference terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" and the like mean that the specific features, structures, materials, or characteristics represented in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. Moreover, the specific features, structures, materials, or characteristics represented may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples represented in the present disclosure and the features of different embodiments or examples, unless they are mutually contradictory.

[0031] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the representation of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0032] In order to clearly describe the present disclosure, components not related to the description are omitted, and the same reference numerals are given to the same or similar components throughout the specification.

[0033] Throughout the specification, when a device is said to be "connected" to another device, this includes not only the case of "direct connection" but also the case of "indirect connection" by placing other elements therebetween. In addition, when a device is said to "include" a certain component, unless otherwise stated, it does not exclude other components, but means that other components may be included.

[0034] Although the terms first, second, etc. are used to represent various elements in this article in some examples, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, the first interface and the second interface, etc. are represented. Moreover, as used in this article, the singular forms "one", "one" and "the" are intended to also include plural forms, unless there is an opposite indication in the context. It should be further understood that the terms "comprising", "including" indicate the existence of features, steps, operations, elements, modules, projects, kinds, and / or groups, but do not exclude the existence, occurrence or addition of one or more other features, steps, operations, elements, modules, projects, kinds, and / or groups. The terms "or" and "and / or" used herein are interpreted as inclusive, or mean any one or any combination. Therefore, "A, B or C" or "A, B and / or C" means "any of the following: A; B; C; A and B; A and C; B and C; A, B and C". Exceptions to this definition occur only when a combination of elements, functions, steps or operations are inherently mutually exclusive in some manner.

[0035] The technical terms used herein are only used to refer to specific embodiments and are not intended to limit the present disclosure. The singular form used herein also includes the plural form unless the sentence clearly indicates the contrary meaning. The meaning of "including" used in the specification is to specify specific characteristics, regions, integers, steps, operations, elements and / or components, and does not exclude the existence or addition of other characteristics, regions, integers, steps, operations, elements and / or components.

[0036] Terms indicating relative space, such as "below" and "above", may be used to more easily describe the relationship of one device illustrated in the drawings relative to another device. Such terms refer not only to the meaning indicated in the drawings, but also to other meanings or executions of the device in use. For example, if the device in the drawings is turned over, a device that was described as being "below" other devices is described as being "above" other devices. Therefore, the exemplary term "below" includes both above and below. The device can be rotated 90° or other angles, and the terms indicating relative space are interpreted accordingly.

[0037] Although not defined differently, all terms, including technical and scientific terms used herein, have the same meaning as those generally understood by those skilled in the art to which the present disclosure belongs. Terms defined in commonly used dictionaries are additionally interpreted as having meanings consistent with relevant technical literature and the message of the present disclosure, and shall not be overly interpreted as ideal or very formal meanings unless defined.

[0038] Figure 1 A flow chart showing a method for manufacturing a solar cell according to an embodiment of the present disclosure is shown in FIG. Figure 1As shown, the solar cell manufacturing method includes the following steps:

[0039] Step 110: forming a doped emitter layer on the front side of the silicon wafer;

[0040] Step 120: forming a first passivation layer on the emitter layer and forming a second passivation layer on the back side of the silicon wafer;

[0041] Step 130: before or after forming the first passivation layer and the second passivation layer, laser bombard the emitter layer to activate doping.

[0042] Using this embodiment, compared with the related art using high temperature diffusion technology, the embodiment of the present disclosure proposes to use a laser bombardment method to activate the emitter layer through doping, which reduces the emitter saturation current density and surface heating while providing enhanced conductivity and implicit open circuit voltage.

[0043] In the embodiment of the present disclosure, before step 110, the surface of the silicon wafer may be subjected to texturing treatment.

[0044] In some embodiments, the silicon wafer is textured to form a velvet surface or a surface texture structure (eg, a pyramid structure). The texture treatment may be carried out by chemical etching, laser etching, mechanical method, plasma etching, etc., which are not limited here.

[0045] For example, a wet texturing process may be selected but not limited to be used for texturing of a P-type silicon wafer. When the P-type silicon wafer is a P-type single crystal silicon substrate, an alkaline solution such as a potassium hydroxide solution may be used for texturing; when the P-type substrate is a P-type polycrystalline silicon substrate, an acidic solution such as a hydrofluoric acid solution may be used for texturing. In addition, a small amount of a texturing additive may be added to the above acidic solution or alkaline solution.

[0046] In this embodiment, the surface of the silicon substrate is provided with a velvet structure by texturing, thereby generating a light trapping effect, increasing the amount of light absorbed by the solar cell, and thus improving the conversion efficiency of the solar cell.

[0047] Optionally, before the texturing process, a step of cleaning the silicon wafer may be included to remove metal and organic pollutants on the surface.

[0048] Taking Topcon cells as an example, the front side of the N-type silicon wafer (the surface facing the sun) is doped with boron to form a P-type doped layer (P+ layer). Then, a boron-doped amorphous silicon layer is deposited on the surface of the P-type doped layer. In some embodiments, the boron concentration in the P-type doped layer is less than the boron concentration in the boron-doped amorphous silicon layer.

[0049] In the embodiments of the present disclosure, Figure 2As shown, a silicon wafer 1 is provided, a first silicon oxide layer 2 is deposited on the front side of the silicon wafer 1, and a passivation contact layer 3 is deposited on the back side of the silicon wafer 1;

[0050] refer to Figure 3 , forming an emitter layer 4 on the first silicon oxide layer 2, wherein the emitter layer 4 covers the first silicon oxide layer 2;

[0051] refer to Figure 4 , a first passivation layer 5 is formed on the emitter layer 4 and a second passivation layer 6 is formed on the side of the passivation contact layer 3 facing away from the silicon wafer 1 , then the second passivation layer 6 is located on the side of the passivation contact layer 3 facing away from the silicon wafer 1 .

[0052] In the TOPCon cell, a passivation contact layer 3 is deposited on the back of the cell, which can passivate the metal contact area on the back of the cell, reduce the recombination of photogenerated carriers of the solar cell in the metal contact area on the back of the cell, and thus improve the cell performance.

[0053] In the disclosed embodiment, atmospheric pressure chemical vapor deposition (APCVD) is used to deposit the first silicon oxide layer 2 on the front side of the silicon wafer 1. APCVD refers to a chemical vapor deposition method performed under atmospheric pressure, which is the method originally used for chemical vapor deposition. The system required for this process is simple, the reaction speed is fast, and the deposition rate is high.

[0054] In the embodiment of the present disclosure, a passivation contact layer 3 is deposited on the back side of the silicon wafer 1, specifically comprising the following steps:

[0055] Depositing a second silicon oxide layer 31 on the back side of the silicon wafer 1;

[0056] Using SiH4, O2 and B2H6 as precursors, amorphous silicon is deposited on the side of the second silicon oxide layer 31 facing away from the silicon wafer 1. The amorphous silicon is crystallized during laser bombardment to be converted into a polysilicon layer 32. The second silicon oxide layer 31 and the polysilicon layer 32 constitute a passivation contact layer 3.

[0057] The second silicon oxide layer 31 may refer to the method for forming the first silicon oxide layer 2 , and is not limited here.

[0058] The second silicon oxide layer 31 serves as a tunneling oxide layer and together with the polysilicon layer 32 constitutes a passivation contact layer 3, which can passivate the metal contact area on the back of the battery, reduce the recombination of photogenerated carriers of the solar cell in the metal contact area on the back of the battery, and thus improve the battery performance.

[0059] Among them, intrinsic amorphous silicon can be deposited using low-pressure chemical vapor deposition (LPCVD) or plasma enhanced chemical vapor deposition (PECVD) technology, and then the intrinsic amorphous silicon can be crystallized into phosphorus-doped polycrystalline silicon through laser bombardment. Laser bombardment can achieve crystallization and doping activation of highly doped amorphous silicon.

[0060] In the embodiment of the present disclosure, a doped emitter layer is formed on the front side of a silicon wafer, specifically comprising the following steps:

[0061] The emitter layer 4 is deposited on the front side of the silicon wafer 1 using PH3, O2 and SiH4 as precursors.

[0062] In this way, the emitter layer 4 is doped with phosphorus, and when the laser is bombarded, the phosphorus diffuses and becomes activated.

[0063] In another embodiment, boron nitride (BN 2 ) and boron trichloride (BCI 3 ) as a precursor, an emitter 4 is deposited on the front side of the silicon wafer 1. In this way, the emitter 4 is doped with boron, and when the laser is bombarded, the boron diffuses and activates.

[0064] In a corresponding embodiment, the doping type in the emitter 4 is related to the doping type of the silicon wafer 1 , so that a PN junction is formed between the emitter 4 and the silicon wafer 1 .

[0065] In the embodiment of the present disclosure, the laser irradiation energy range during the laser bombardment process is: 0.3~0.4J / cm 2 , which includes two endpoints 0.3J / cm 2 and 0.4J / cm 2 If the laser irradiation energy is too large, such as more than 0.4J / cm 2 , which is not conducive to passivation, and the laser irradiation energy is too small, such as less than 0.3J / cm 2 , then the heavy doping effect will not be achieved.

[0066] Optionally, the laser irradiation energy range during the laser bombardment process is: 0.38 J / cm 2 .

[0067] In the embodiment of the present disclosure, if the emitter layer 4 is laser bombarded after the first passivation layer 5 and the second passivation layer 6 are formed, the laser passes through the first passivation layer 5 and acts on the emitter layer 4, which can not only activate the doping in the emitter layer 4 to crystallize it, but also improve the passivation effect of the first passivation layer 5 and the second passivation layer 6.

[0068] In an embodiment of the present disclosure, a first passivation layer is formed on the emitter layer and a second passivation layer is formed on the back side of the silicon wafer, including:

[0069] A first passivation layer 5 is formed on the emitter layer 4 and a second passivation layer 6 is formed on the back side of the silicon wafer 1 by using a plasma enhanced chemical vapor deposition (PECVD) method, and high temperature annealing is performed.

[0070] Through high temperature annealing, the adhesion of the first passivation layer 5 and the second passivation layer 6 can be improved, and their stability can be improved.

[0071] Refer to the table below for the comparison of sheet resistance and iVoc using laser blasting and conventional high temperature annealing:

[0072] type Sheet resistance (kohm / sq) ivoc(mV) Control group (high temperature annealing) 5.9 700 Example 1 6.1 703 Example 2 5.8 699

[0073] It can be seen from Example 1 that the ivoc value and the sheet resistance value are higher than those of the control group. Compared with Example 2, it can be seen from Example 1 that, in combination with the foregoing, a good passivation effect can be achieved by selecting a suitable laser irradiation energy.

[0074] In the embodiment of the present disclosure, the first passivation layer 5 and the second passivation layer 6 can be an aluminum oxide passivation layer or a silicon nitride layer or a stacked SiNx film, a SiNx / SiOx stack, a SiNx / AlOx stack or a combination of the three films, which is not limited here.

[0075] The above embodiments are merely illustrative of the principles and effects of the present disclosure, and are not intended to limit the present disclosure. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present disclosure. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present disclosure shall still be covered by the claims of the present disclosure.

Claims

1. A method for manufacturing a solar cell, characterized in that: include: forming a doped emitter layer on the front side of the silicon wafer; forming a first passivation layer on the emitter layer and forming a second passivation layer on the back side of the silicon wafer; After forming the first passivation layer and the second passivation layer, the emitter layer is laser bombarded to activate doping. The laser irradiation energy range of the laser bombardment process is: 0.3-0.4 J / cm 2 ; Before forming a doped emitter layer on the front side of the silicon wafer, depositing a first silicon oxide layer on the front side of the silicon wafer, wherein the emitter layer covers the first silicon oxide layer; Before forming the second passivation layer on the back side of the silicon wafer, a passivation contact layer is deposited on the back side of the silicon wafer, wherein the second passivation layer is located on a side of the passivation contact layer facing away from the silicon wafer; The step of depositing a passivation contact layer on the back side of the silicon wafer comprises: Depositing a second silicon oxide layer on the back side of the silicon wafer; Using SiH4, O2 and B2H6 as precursors, amorphous silicon is deposited on the side of the second silicon oxide layer facing away from the silicon wafer. The amorphous silicon is crystallized during the laser bombardment to be converted into a polycrystalline silicon layer. The second silicon oxide layer and the polycrystalline silicon layer constitute the passivation contact layer.

2. The method for manufacturing a solar cell according to claim 1, characterized in that: A doped emitter layer is formed on the front side of the silicon wafer, including: The emitter layer is deposited on the front side of the silicon wafer using PH3, O2 and SiH4 as precursors.

3. The method for manufacturing a solar cell according to claim 1, characterized in that: A doped emitter layer is formed on the front side of the silicon wafer, including: The emitter was deposited on the front side of the silicon wafer using BN2 and BCI3 as precursors.

4. The method for manufacturing a solar cell according to claim 1, characterized in that: The laser pulse overlap rate during the laser bombardment process is 40%-60%.

5. The method for manufacturing a solar cell according to claim 1, characterized in that: The laser irradiation energy range during the laser bombardment is: 0.38J / cm 2 .

6. The method for manufacturing a solar cell according to claim 1, characterized in that: The forming of a first passivation layer on the emitter layer and a second passivation layer on the back side of the silicon wafer comprises: A first passivation layer is formed on the emitter layer and a second passivation layer is formed on the back side of the silicon wafer by using a plasma enhanced chemical vapor deposition method, and high temperature annealing is performed.