Spherical alumina powder, resin composition, heat dissipation material
By adjusting the particle size distribution of spherical alumina powder and the viscosity ratio of the resin composition, liquid cross-linking is suppressed, and the problem of increased viscosity when ceramic powder is highly filled is solved, and good fluidity and high filling rate of spherical alumina powder are achieved. Reduces adverse factors in molding processing.
Patent Information
- Application Number
- CN202180066947.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2021-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-09-24
AI Technical Summary
When existing ceramic powders are highly filled in silicone resins, the viscosity of the material increases, which increases the adverse factors in molding and processing, making it difficult to achieve good fluidity and high filling rate.
By adjusting the particle size distribution of spherical alumina powder and the viscosity ratio of the resin composition, the maximum particle size is in the range of 35 to 70 μm, the frequency is 5 to 15%, and the frequency accumulation value within the range of 1 to 20 μm is 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 35 to 70 μm, the frequency is 3 to 3 to 3 to 3 17% by volume, the viscosity ratio was controlled to be above 0.85, liquid crosslinking was inhibited, and high fluidity was maintained.
The good fluidity and high filling rate of spherical alumina powder are achieved, the viscosity of the material is reduced, the adverse factors in molding are avoided, and the fluidity and moldability of the material are improved.
Smart Images

Figure BDA0004151581400000151
Abstract
Description
Technical Field
[0001] The invention relates to spherical alumina powder, resin composition and heat dissipation material. Background Art
[0002] In recent years, in order to meet the requirements of small, light and high-performance electronic equipment, the miniaturization, thinness and narrow pitch of semiconductor packaging have been rapidly developed. In addition, surface mounting suitable for high-density mounting on wiring substrates has also become the mainstream mounting method. As a result, with the development of semiconductor packaging and its mounting method, the performance of heat dissipation materials is also required to be improved, and ceramic powders, especially spherical alumina powders highly filled in silicone resins, have been studied in depth. The problem with highly filled ceramic powders is that the viscosity of the material increases, which increases the undesirable factors in the molding process.
[0003] In order to solve this problem, improvements have been made from the resin and ceramic powder aspects. As improvements in ceramic powder, for example, a method of increasing the Wardle sphericity to 0.7 to 1.0 (Patent Document 1), a method of setting the slope of the straight line shown in the Rosin-Rammler line graph to 0.6 to 0.95, a method of expanding the particle size distribution (Patent Document 2), a method of providing multiple peaks in the particle size distribution to form a multimodal particle size distribution, and making the ceramic powder close to the most densely packed structure (Patent Document 3), etc., are still insufficient. If the filling rate is increased, the viscosity of the material will increase sharply.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 3-066151
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 6-080863
[0008] Patent Document 3: Japanese Patent Application Laid-Open No. 8-003365 Summary of the invention
[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a practical spherical alumina powder having good fluidity.
[0010] The present inventors have conducted intensive studies to solve the above problems, and as a result, have found that the above problems can be solved by the present invention described below, thereby completing the present invention.
[0011] That is, the present invention is as follows.
[0012] [1] A spherical alumina powder, wherein in a particle size distribution measured by a laser diffraction scattering particle size distribution analyzer, the maximum particle size showing a maximum peak is in the range of 35 to 70 μm, the frequency of the maximum particle size is 5 to 15%, and the frequency accumulation value of each of the particle sizes at 20 points obtained by dividing the particle size range of 1 to 20 μm into 19 equal parts is 3 to 17% by volume, wherein the viscosity of a resin composition X containing the spherical alumina powder and vinyl polymethylsiloxane and containing 88.1% by mass of the spherical alumina powder is denoted as V X The resin composition X contains 79.3% by mass of spherical alumina powder and 8.8% by mass of test alumina powder, and the viscosity of the resin composition Y which is the same as the resin composition X is V Y When their ratio is V Y / V X is 0.85 or more, wherein the vinyl-containing polymethylsiloxane and the test spherical alumina powder meet the following conditions:
[0013] [About vinyl methicone],
[0014] Viscosity (23°C JIS K 6209) is 1.1 to 1.3 Pa·s.
[0015] [About the alumina powder used in the test],
[0016] (1) Average particle size (D50) 6.8 μm,
[0017] (2) Specific surface area: 0.4m 2 / g.
[0018] [2] A resin composition comprising a resin and the alumina powder described in [1].
[0019] [3] A heat dissipation material comprising the resin composition described in [2].
[0020] According to the present invention, it is possible to provide a practical spherical alumina powder having good fluidity. DETAILED DESCRIPTION
[0021] Hereinafter, an embodiment of the present invention (this embodiment) will be described in detail.
[0022] [Spherical alumina powder]
[0023] The spherical alumina powder involved in the present embodiment has a particle size distribution measured by a laser diffraction scattering particle size distribution analyzer, in which the maximum particle size of the maximum peak is in the range of 35 to 70 μm, and the frequency of the maximum particle size is 5 to 15%. In addition, for the particle sizes of 20 points obtained by dividing the particle size range of 1 to 20 μm into 19 equal parts, the cumulative value of their respective frequencies is 3 to 17 volume %.
[0024] If the maximum particle size is outside the above range, rolling resistance increases and the viscosity of the resin composition containing the spherical alumina powder increases. The maximum particle size is preferably in the range of 35 to 70 μm.
[0025] If the frequency of the maximum particle size is not within the range of 5 to 15%, rolling resistance increases and the viscosity of the resin composition containing the spherical alumina powder increases. The frequency of the maximum particle size is preferably within the range of 7 to 11%.
[0026] Furthermore, the spherical alumina powder involved in this embodiment is that the cumulative value of each frequency of 20 points of particle diameter (20 points of particle diameters of 1 μm, 2 μm, 3 μm, ..., 20 μm) obtained by dividing the particle diameter range into 19 equal parts within the particle diameter range of 1 to 20 μm is 3 to 17% by volume. If this condition is not satisfied, the inhibitory effect of liquid crosslinking is reduced, and the viscosity of the resin composition containing the spherical alumina powder increases. The cumulative value of the above frequency in the particle diameter range of 1 to 20 μm is preferably 5 to 14% by volume.
[0027] Here, liquid crosslinking is explained. Usually, if the powder is densely filled, liquid crosslinking occurs between the powder particles under the influence of moisture on the particle surface. If liquid crosslinking occurs, the viscosity increases, and the fluidity as a resin composition decreases. Based on this phenomenon, it is speculated that in the present invention, the above-mentioned small-particle-size spherical alumina powder with a particle size in the range of 1 to 20 μm exists between or in the gaps between the spherical alumina powder particles with the largest particle size showing the maximum peak as the main component, thereby suppressing liquid crosslinking between the powders and achieving high fluidity even in a dense powder state.
[0028] The spherical alumina powder according to the present embodiment is prepared by setting the viscosity of the resin composition X containing the spherical alumina powder and vinyl polymethylsiloxane and containing 88.1% by mass of the spherical alumina powder to V. X The resin composition X contains 79.3% by mass of spherical alumina powder and 8.8% by mass of test alumina powder, and the viscosity of the resin composition Y which is the same as the resin composition X is V Y When their ratio is V Y / V XThe powder has a viscosity of 0.85 or more, wherein the vinyl-containing polymethylsiloxane and the test spherical alumina powder satisfy the following conditions:
[0029] [About vinyl methicone]
[0030] Viscosity (23℃JIS K 6209) 1.1~1.3Pa·s;
[0031] [About the Alumina Powder for Testing]
[0032] (1) Average particle size (D50) 6.8 μm
[0033] (2) Specific surface area: 0.4m 2 / g.
[0034] As the vinyl-containing polymethylsiloxane, a liquid with a trade name of YE5822A (viscosity of 1.2 Pa·s) manufactured by Momentive Performance Materials Japan LLC is preferably used. As the alumina powder for testing, a liquid with a trade name of DAW-05 manufactured by Denka is preferably used.
[0035] Here, the resin composition Y has a particle size distribution closer to the closest packed structure, and the viscosity V of the resin composition X is X The viscosity V of the resin composition Y Y Ratio (V Y / V X ) is 0.85 or more, which can be said to be a particle size distribution that effectively inhibits liquid crosslinking between particles. Y / V X If the value is less than 0.85, the particle size distribution cannot suppress the increase in viscosity due to liquid crosslinking. Y / V X It is preferably 0.9 to 1.1.
[0036] In order to make V Y / V X Within the above range, for example, among the respective frequencies of 20 particle sizes obtained by dividing the particle size range from 1 to 20 μm into 19 equal parts (20 particle sizes of 1 μm, 2 μm, 3 μm, ..., 20 μm), preferably, the frequencies of at least 6 particle sizes are respectively greater than 0.1%, and among the 20 particle sizes, more preferably, the frequencies of at least 9 particle sizes are respectively greater than 0.1%.
[0037] The maximum peak value in this specification is as described above, and is measured by a laser diffraction scattering particle size distribution analyzer, and can be specifically measured and calculated according to the method described in the examples.
[0038] The cumulative value of the frequency of the particle size region within the peak having the maximum peak is preferably 70% by volume or more, more preferably 75 to 90% by volume. When the cumulative value of the frequency is 70% by volume or more, an increase in viscosity can be prevented.
[0039] Here, the range of the peak with the maximum peak is the range from a particle diameter of 20 μm to a frequency minimum value via the maximum peak, and the particle diameter is preferably in the range of 20 to 100 μm. In addition, the particle diameter when the frequency is the maximum in the above range is the maximum particle diameter.
[0040] The average particle size of the spherical alumina powder according to the present embodiment is preferably 35 to 70 μm, more preferably 40 to 60 μm. By setting the average particle size to 35 to 70 μm, an increase in viscosity can be prevented.
[0041] Here, the above average particle size is the cumulative 50% diameter (D50) of the volume basis measured by a laser diffraction scattering particle size distribution measuring instrument, which can be measured and calculated by the method described in the examples. In addition, the cumulative 10% diameter (D10) refers to the cumulative 10% diameter of the volume basis, and the cumulative 90% diameter (D90) refers to the cumulative 90% diameter of the volume basis.
[0042] The average sphericity of the spherical alumina powder according to the present embodiment is preferably 0.9 or more, and more preferably 0.92 to 1. By setting the average sphericity to 0.9 or more, an increase in viscosity can be prevented.
[0043] Here, the above average sphericity can be measured and calculated by the method described in Examples.
[0044] In addition, the specific surface area is preferably 0.1 to 0.4 m 2 / g, more preferably 0.2 to 0.3 m 2 / g. By making the specific surface area 0.1 to 0.4 m 2 / g, can prevent the increase of viscosity.
[0045] Here, the above-mentioned specific surface area is a value based on the BET method and can be measured and calculated by the BET one-point method.
[0046] The spherical alumina powder according to the present embodiment can be produced, for example, as follows.
[0047] First, the alumina raw material powder as a raw material is preferably alumina powder or aluminum hydroxide powder.
[0048] Afterwards, the alumina raw material powder having an average particle size approximately the same as the desired maximum particle size is put into a high-temperature flame formed by a fuel gas such as hydrogen, natural gas, acetylene gas, propane gas, butane, LPG, etc., and is melted and spheroidized to produce the first spherical alumina powder.
[0049] Similarly, a second spherical alumina powder is produced by melting and spheroidizing alumina raw material powder having an average particle size of 1 to 20 μm.
[0050] The average sphericity and specific surface area of the spherical alumina powder can be adjusted by controlling at least one of the temperature in the furnace for forming the high-temperature flame, the particle size and the input amount of the alumina raw material powder.
[0051] Next, the particle size distribution of the first spherical alumina powder is adjusted to a desired range using a sieve or a precision wind classifier, etc. Similarly, the particle size distribution of the second spherical alumina powder is adjusted to a desired range using a sieve or a precision wind classifier, etc.
[0052] At this time, the desired range means that among the respective frequencies of the particle sizes of 20 points obtained by dividing the particle size range of 1 to 20 μm into 19 equal parts, the respective frequencies of the particle sizes of at least 6 points are in the range of 0.1% or more, the maximum particle size showing the maximum peak is in the range of 35 to 70 μm, and the frequency of the maximum particle size is in the range of 5 to 15%, etc.
[0053] It should be noted that the shape of the peak of the particle size distribution can be made sharper or wider by adjusting the feed amount of the precise air classification and the like.
[0054] In particular, when V Y / V X When it is above 0.85, among the respective frequencies of 20 particle sizes (20 particle sizes of 1 μm, 2 μm, 3 μm, ..., 20 μm) divided into 19 equal parts within the particle size range of 1 to 20 μm by a precision wind classifier, it is preferred to adjust the respective frequencies of at least 6 particle sizes to above 0.1%.
[0055] [Resin composition, heat dissipation material]
[0056] The resin composition of the present invention contains a resin and the above-mentioned alumina powder of the present invention. In addition, the heat dissipation material of the present invention contains the above-mentioned resin composition of the present invention.
[0057] As the resin, for example, silicone resin, epoxy resin, phenolic resin, melamine resin, urea-formaldehyde resin, unsaturated polyester, fluororesin, polyimide, polyamide-imide, polyetherimide and other polyamides, polybutylene terephthalate, polyethylene terephthalate and other polyesters, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyarylether sulfone, polycarbonate, maleimide-modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, etc. can be used.
[0058] Among these, the resin used as the heat dissipation material is preferably a silicone resin, preferably at least one of an addition reaction type silicone resin and a condensation reaction type silicone resin. In addition, as required, a part of the silicone resin may be replaced with silicone rubber. The silicone rubber is preferably at least one of an addition reaction type silicone rubber and a peroxide vulcanized silicone rubber.
[0059] Any of these silicone resins and silicone rubbers preferably has an average composition formula of R 1 n SiO (4-n) / 2 (R in the formula 1 are the same or different unsubstituted or substituted monovalent hydrocarbon groups, and n is a positive number of 1.98 to 2.02. ) is an organopolysiloxane as a main component.
[0060] Specific examples of silicone resins include one-component silicones having both a vinyl group and an H-Si group in one molecule, and two-component silicones having a vinyl-containing polysiloxane at the end or side chain. For sale, products such as those produced by Toshiba Silicones are named "XE14-8530", "TSE-3062" and "YE5822".
[0061] The resin composition or heat dissipation material of the present invention can be mixed with the following components as needed. That is, as the low stress agent, there can be mentioned rubbery substances such as silicone rubber, polysulfide rubber, acrylic rubber, butadiene rubber, styrene block copolymers, saturated elastomers, various thermoplastic resins, and resins obtained by partially or completely modifying epoxy resins and phenolic resins with aminosiloxane, epoxysiloxane, alkoxysiloxane, etc.
[0062] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino silanes such as aminopropyltriethoxysilane, ureidopropyltriethoxysilane, phenylaminosilane, and N-phenylaminopropyltrimethoxysilane, hydrophobic silane compounds such as phenyltrimethoxysilane, methyltrimethoxysilane, and octadecyltrimethoxysilane, and mercaptosilane.
[0063] Examples of the surface treatment agent include Zr chelate compounds, titanate coupling agents, and aluminum-based coupling agents.
[0064] Examples of the flame retardant include halogenated epoxy resins and phosphorus compounds, and examples of the colorant include carbon black, iron oxide, dyes, pigments, and the like.
[0065] As flame retardant additives, Sb 2 O 3 , Sb2 O 4 , Sb 2 O 5 wait.
[0066] Examples of the release agent include natural waxes, synthetic waxes, metal salts of linear fatty acids, amides, esters, and paraffin waxes.
[0067] The content of the spherical alumina powder of the present invention in the resin composition or the heat dissipating material is preferably 50 to 95% by mass. By setting the content within the above range, desired heat resistance and moldability can be obtained.
[0068] The resin composition or heat dissipation material of this embodiment can be manufactured by mixing the above-mentioned materials in a specified amount using a stirrer or a Henschel mixer, kneading with a heating roll, a kneader, a single-axis or double-axis extruder, etc., and then appropriately pulverizing the obtained product after cooling.
[0069] It should be noted that when preparing a resin composition or a heat dissipation material, by subjecting the spherical alumina powder of the present invention to surface treatment with the above-mentioned silane coupling agent or the like, the water absorption rate of the powder can be reduced, the strength of the resin composition can be increased, the interface resistance between the resin and the powder can be further reduced, and the thermal conductivity can be further improved.
[0070] The heat dissipation material of this embodiment is preferably a thin molded body such as a sheet, and its processing method is a conventionally known method, such as a doctor blade method, a coating method using a notch wheel coater, an extrusion method, etc. The thickness of the sheet heat dissipation material is preferably 0.3 mm or more.
[0071] Example
[0072] Hereinafter, the present invention will be described in more detail by way of Examples and Comparative Examples, but the present invention is not limited to the following Examples without departing from the gist of the present invention.
[0073] [Example 1]
[0074] (Preparation of the first spherical alumina powder)
[0075] The alumina powder was put into a flame formed by LPG and oxygen, spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 45 μm.
[0076] (Production of the Second Spherical Alumina Powder)
[0077] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 6 μm.
[0078] In addition, the average particle size and the average sphericity were measured in the following manner (the same for the following Examples and Comparative Examples).
[0079] (Method for measuring average particle size)
[0080] The average particle size (volume basis) of the spherical alumina powder was measured by a laser diffraction scattering method (Microtrac (manufactured by Nikkiso, trade name “MT3300EX II”)).
[0081] (Method for measuring average sphericity)
[0082] The average sphericity of spherical alumina powder is measured using a flow particle image analyzer called "FPIA-3000" produced by Sysmex Corporation in the following manner. The projected area (A) and perimeter (PM) of the particle are measured from the particle image. Let the area of a perfect circle with respect to the perimeter (PM) be (B), and the sphericity of the particle can be expressed as A / B. Therefore, assuming a perfect circle with the same perimeter as the perimeter (PM) of the sample particle, PM = 2πr, B = πr 2 , so B = π × (PM / 2π) 2 , the sphericity of each particle can be calculated as roundness = A / B = A×4π / (PM) 2 The average sphericity is measured for 100 or more particles selected at random, and the square of the average value is taken as the average sphericity. A measurement solution is prepared by adding 20 ml of distilled water and 10 ml of propylene glycol to 0.1 g of a sample and performing ultrasonic dispersion treatment for 3 minutes.
[0083] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 5:95 to prepare the spherical alumina powder of Example 1 (average particle size of 45 μm, specific surface area of 0.2 m 2 / g).
[0084] The particle size distribution (particle size and frequency) of the spherical alumina powder of Example 1 was measured by laser diffraction scattering method. The above-mentioned Microtrac was used as a particle size distribution measuring instrument.
[0085] The results are shown in Table 1 below.
[0086] The spherical alumina powder prepared above is added to vinyl-containing polymethylsiloxane (produced by Momentive Performance Materials Japan LLC, trade name YE5822A liquid) to a concentration of 65 volume % (88.1 mass %) in the resin composition, and then stirred and degassed to prepare resin composition X.
[0087] In addition, resin composition Y was prepared in the same manner as resin composition X except that the content of spherical alumina powder in resin composition X was 79.3 mass % and 8.8 mass % of test alumina powder (manufactured by Denka Co., Ltd., trade name DAW-05) was contained. Viscosity V of resin composition X X With viscosity V Y The viscosity of each was measured at 30°C using a B-type viscometer (manufactured by Toki Kogyo Co., Ltd., trade name "TVB-10"). In addition, their ratio (V Y / V X ). The viscosity V of the resin composition X is shown in the following Table 1. X and V Y / V X In addition, the viscosity is preferably 100 Pa·s or less.
[0088] Here, the vinyl-containing polymethylsiloxane and the test spherical alumina powder have the following properties.
[0089] [About vinyl methicone]
[0090] (1) Viscosity (23°C JIS K 6209) 1.2 Pa·s
[0091] [About the Alumina Powder for Testing]
[0092] (1) Average particle size (D50) 6.8 μm
[0093] (2) Specific surface area: 0.4m 2 / g
[0094] [Example 2]
[0095] (Preparation of the first spherical alumina powder)
[0096] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 44 μm.
[0097] (Production of the Second Spherical Alumina Powder)
[0098] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 4 μm.
[0099] The first spherical alumina powder and the second spherical alumina powder were mixed in a volume ratio of 15:85 to prepare the spherical alumina powder of Example 2 (average particle size of 40 μm, specific surface area of 0.3 m2 / g).
[0100] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0101] [Example 3]
[0102] (Preparation of the first spherical alumina powder)
[0103] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 42 μm.
[0104] (Production of the Second Spherical Alumina Powder)
[0105] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0106] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 5:95 to prepare the spherical alumina powder of Example 3 (average particle size of 43 μm, specific surface area of 0.2 m 2 / g).
[0107] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0108] [Example 4]
[0109] (Preparation of the first spherical alumina powder)
[0110] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 55 μm.
[0111] (Production of the Second Spherical Alumina Powder)
[0112] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 7 μm.
[0113] The first spherical alumina powder and the second spherical alumina powder were mixed in a volume ratio of 15:85 to prepare the spherical alumina powder of Example 4 (average particle size of 52 μm, specific surface area of 0.3 m2 / g).
[0114] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0115] [Example 5]
[0116] (Preparation of the first spherical alumina powder)
[0117] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 37 μm.
[0118] (Production of the Second Spherical Alumina Powder)
[0119] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 6 μm.
[0120] The first spherical alumina powder and the second spherical alumina powder were mixed in a volume ratio of 15:85 to prepare the spherical alumina powder of Example 5 (average particle size of 36 μm, specific surface area of 0.2 m 2 / g).
[0121] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0122] [Example 6]
[0123] (Preparation of the first spherical alumina powder)
[0124] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 56 μm.
[0125] (Production of the Second Spherical Alumina Powder)
[0126] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 4 μm.
[0127] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 5:95 to prepare the spherical alumina powder of Example 6 (average particle size of 55 μm, specific surface area of 0.2 m2 / g).
[0128] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0129] [Example 7]
[0130] (Preparation of the first spherical alumina powder)
[0131] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 49 μm.
[0132] (Production of the Second Spherical Alumina Powder)
[0133] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 3 μm.
[0134] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 10:90 to prepare the spherical alumina powder of Example 7 (average particle size of 44 μm, specific surface area of 0.20 m 2 / g).
[0135] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0136] [Example 8]
[0137] (Preparation of the first spherical alumina powder)
[0138] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 56 μm.
[0139] (Production of the Second Spherical Alumina Powder)
[0140] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0141] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 20:80 to prepare the spherical alumina powder of Example 8 (average particle size of 52 μm, specific surface area of 0.2 m2 / g).
[0142] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0143] [Comparative Example 1]
[0144] (Preparation of the first spherical alumina powder)
[0145] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 54 μm.
[0146] (Production of the Second Spherical Alumina Powder)
[0147] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0148] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 20:80 to prepare the spherical alumina powder of Comparative Example 1 (average particle size of 48 μm, specific surface area of 0.2 m 3 / g).
[0149] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0150] [Comparative Example 2]
[0151] (Preparation of the first spherical alumina powder)
[0152] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 45 μm.
[0153] (Production of the Second Spherical Alumina Powder)
[0154] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0155] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 2:98 to prepare the spherical alumina powder of Comparative Example 2 (average particle size of 44 μm, specific surface area of 0.1 m3 / g).
[0156] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0157] [Comparative Example 3]
[0158] (Preparation of the first spherical alumina powder)
[0159] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 45 μm.
[0160] (Production of the Second Spherical Alumina Powder)
[0161] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0162] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 20:80 to prepare the spherical alumina powder of Comparative Example 3 (average particle size of 41 μm, specific surface area of 0.4 m 3 / g).
[0163] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0164] [Comparative Example 4]
[0165] (Preparation of the first spherical alumina powder)
[0166] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 60 μm.
[0167] (Production of the Second Spherical Alumina Powder)
[0168] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0169] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 5:95 to prepare the spherical alumina powder of Comparative Example 4 (average particle size of 59 μm, specific surface area of 0.2 m3 / g).
[0170] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0171] [Comparative Example 5]
[0172] (Preparation of the first spherical alumina powder)
[0173] The alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain an alumina powder with an average sphericity of 0.92 and an average particle size of 44 μm.
[0174] (Production of the Second Spherical Alumina Powder)
[0175] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 5 μm.
[0176] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 15:85 to prepare the spherical alumina powder of Comparative Example 5 (average particle size of 39 μm, specific surface area of 0.2 m 2 / g).
[0177] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0178] [Comparative Example 6]
[0179] (Preparation of the first spherical alumina powder)
[0180] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 46 μm.
[0181] (Production of the Second Spherical Alumina Powder)
[0182] Alumina powder was put into a flame formed by LPG and oxygen to be spheroidized, and then classified by cyclone classification to obtain alumina powder with an average sphericity of 0.92 and an average particle size of 10 μm.
[0183] The first spherical alumina powder and the second spherical alumina powder were mixed at a volume ratio of 15:85 to prepare the spherical alumina powder of Comparative Example 6 (average particle size of 42 μm, specific surface area of 0.2 m3 / g).
[0184] Using this spherical alumina powder, a resin composition was prepared in the same manner as in Example 1, and the viscosity of the prepared resin composition was measured. The results are shown in Table 1 below.
[0185] [Table 1]
[0186]
[0187] [Industrial Applicability]
[0188] The spherical alumina powder of the present invention is suitable as a filler for a thermally conductive resin composition. In addition, the resin composition of the present invention can be used as a heat dissipation member for heat countermeasures in personal computers, automobiles, mobile electronic devices, household appliances, and the like.
Claims
1. A spherical aluminum oxide powder having a maximum peak value of 35 to 70 μm in a particle size distribution measured by a laser diffraction scattering particle size distribution measuring instrument. μ m range, the frequency of the maximum particle size is 5-15%, For particle sizes between 1 and 20 μ The cumulative value of the frequency of the particle diameters at 20 points obtained by dividing the range of m into 19 equal parts is 3 to 17% by volume. in, The viscosity of the resin composition X containing the spherical alumina powder and vinyl polymethylsiloxane and containing 88.1% by mass of the spherical alumina powder is defined as V. X The resin composition X contained 79.3% by mass of spherical alumina powder and 8.8% by mass of test alumina powder, and the viscosity of the resin composition Y which was the same as the resin composition X was V Y When their ratio is V Y / V X is 0.85 or more, wherein the vinyl-containing polymethylsiloxane and the test alumina powder meet the following conditions: For vinyl-containing polymethylsiloxane, The viscosity is 1.1 to 1.3 Pa·s, where the viscosity is the viscosity at 23° C. based on JIS K 6209. For the alumina powder used in the test, (1) Average D50 particle size is 6.8 μ m, (2) Specific surface area is 0.4m 2 / g.
2. A resin composition comprising a resin and the spherical alumina powder according to claim 1.
3. A heat dissipation material comprising the resin composition according to claim 2.
Citation Information
Patent Citations
Alumina powder, process for production of the same, and resin compositions containing the same
CN102007073A
Amorphous siliceous powder, process for production thereof, resin composition, and semiconductor encapsulation material
CN102066254A
Method for producing spherical aluminum powder
CN102249276A
Spherical alumina powder and resin composition including same
CN106660817A
Alumina particle
CN111902363A