Resin molding material, molded body, and method for producing the molded body
By using high-content soft magnetic particles and liquid silicone compounds in resin molding materials, combined with thermosetting resin, the trade-off between magnetic permeability and fillability is solved, and a resin molding material with high magnetic permeability and excellent fillability is achieved , avoid shrinkage and pollution of molded objects.
Patent Information
- Application Number
- CN202180068192.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-05
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-09-30
AI Technical Summary
In resin molding materials, there is a trade-off between improving magnetic permeability and filling. The high filling amount of soft magnetic particles will lead to an increase in viscosity, affecting the filling ability during molding, and the leakage of organic silicon compounds in the prior art will contaminate Molded products and molds.
Using more than 96% of soft magnetic particles and organic silicon compounds that are liquid at room temperature, combined with thermosetting resin, the particle size and amount of silicon compounds are appropriately adjusted to improve magnetic permeability and fillability, while suppressing void and dispersion unevenness. The problem.
High magnetic permeability and excellent mold filling properties are achieved, ensuring the magnetic and mechanical characteristics of the molded body, and avoiding shrinkage and contamination of the molded object.
Smart Images

Figure BDA0004161025160000051 
Figure BDA0004161025160000061 
Figure BDA0004161025160000062
Abstract
Description
Technical Field
[0001] The present invention relates to a resin molding material, a molded body and a method for producing the molded body. Background Art
[0002] Research is actively underway on coils with magnetic cores and outer casings (also called "reactors" or "inductors" depending on the application field) as parts for various electrical and electronic products. In addition, research is also actively underway on magnetic materials with moldability used to make the magnetic cores or outer casings of such coils.
[0003] For example, Patent Document 1 discloses a compound containing a powder containing a metal element, an epoxy resin, and a compound having a siloxane bond. The document states that the compound having a siloxane bond is contained in an amount of 25 parts by mass or more and 45 parts by mass or less relative to 100 parts by mass of the epoxy resin in order to reduce the molding shrinkage of the compound.
[0004] Patent Document 2 discloses a resin molding material comprising magnetic powder whose surface is coated with a predetermined organic silicon compound and a thermosetting resin. This document describes that both a high filling rate in a molded product and high fluidity during molding can be achieved.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2019 / 229960
[0008] Patent Document 2: Japanese Patent Application Publication No. 2020-114939 Summary of the invention
[0009] Technical problem to be solved by the invention
[0010] Here, in the magnetic material obtained from the resin molding material (composition) by transfer molding or compression molding, in order to improve the magnetic properties such as magnetic permeability, it is necessary to highly fill the soft magnetic particles. However, if the filling amount of the soft magnetic particles is increased, the viscosity of the resin molding material increases, which leads to a decrease in the filling property into the mold during the molding such as compression molding. That is, there is a trade-off between the high magnetic permeability of the magnetic material and the improvement of the filling property into the mold.
[0011] In Patent Document 1, the amount of the compound having a siloxane bond added is large, and this compound may bleed out during molding, and may contaminate the surface of the molded product or the surface of the mold.
[0012] Patent Document 2 discloses that a small amount of a predetermined organosilicon compound exists on the surface of the magnetic powder. When the soft magnetic particles are filled in a high amount, the amount of the organosilicon compound between the soft magnetic particles further affects the fluidity. Therefore, the fluidity of the resin molding material in this document still needs to be improved.
[0013] Technical solutions for solving technical problems
[0014] As a result of intensive research, the inventors of the present invention have completed the invention provided below and solved the above-mentioned technical problems. That is, the present invention can be as follows.
[0015] According to the present invention, there is provided a resin molding material for transfer molding or compression molding, comprising:
[0016] (A) Soft magnetic particles;
[0017] (B) an organosilicon compound that is liquid at room temperature (25° C.); and
[0018] (C) thermosetting resin,
[0019] The content of the soft magnetic particles (A) is 96% by mass or more.
[0020] According to the present invention, there is provided a molded body obtained by curing the above-mentioned resin molding material.
[0021] According to the present invention, there is provided a method for manufacturing a molded body, comprising:
[0022] The process of injecting the melt of the resin molding material into a mold using a transfer molding device; and
[0023] The step of solidifying the above melt.
[0024] According to the present invention, there is provided a method for producing a molded body, comprising the step of compression molding the above-mentioned resin molding material.
[0025] Effects of the Invention
[0026] According to the present invention, it is possible to provide a resin molding material for transfer molding or compression molding, which can obtain a magnetic material having a high magnetic permeability and has excellent filling properties into a mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a cross-sectional view showing the configuration of a structure according to this embodiment. DETAILED DESCRIPTION
[0028] Hereinafter, the embodiments of the present invention will be described using the accompanying drawings. In addition, in all the drawings, the same components are marked with the same reference numerals, and the description is appropriately omitted. Also, for example, unless otherwise specified, "1 to 10" means "above 1" to "below 10".
[0029] The resin molding material for transfer molding or compression molding of this embodiment contains:
[0030] (A) Soft magnetic particles;
[0031] (B) an organosilicon compound; and
[0032] (C) thermosetting resin,
[0033] The content of the soft magnetic particles (A) is 96% by mass or more.
[0034] Thus, it is possible to provide a resin molding material that can obtain a magnetic material having a high magnetic permeability and has excellent filling properties into a mold.
[0035] The resin molding material of this embodiment can be suitably used for transfer molding or compression molding. In addition, as a molding method similar to compression molding, powder pressing molding can be cited.
[0036] Compression molding is to fill the mold with resin molding material, then soften and flow the resin molding material under low pressure, close the mold, and heat and pressurize at a mold temperature of about 150°C and a compression pressure of about 10MPa to form the mold. On the other hand, powder pressing is to fill the mold with resin molding material, form it under a high pressure of about 1,000MPa, and then perform annealing at a high temperature of 500°C or above to remove residual stress.
[0037] Thus, compression molding and powder compacting are molding methods that differ in molding pressure and temperature.
[0038] The resin molding material of the present embodiment is designed to be suitably used for transfer molding or compression molding. Therefore, when the resin molding material is used for powder pressing under high temperature / high pressure conditions as described above, voids or unfilled parts may be generated due to the generation of volatile components, making it difficult to achieve the effect of molding freedom by utilizing the high filling property of the resin molding material of the present embodiment.
[0039] Hereinafter, each component contained in the resin molding material of this embodiment will be described.
[0040] [Soft magnetic particles (A)]
[0041] Soft magnetism refers to ferromagnetism with a small coercive force. Usually, ferromagnetism with a coercive force of 800 A / m or less is called soft magnetism.
[0042] As the constituent material of the soft magnetic particles (A), a metal-containing material having an iron content of 85% or more as a constituent element can be cited. Thus, a metal material having a high iron content as a constituent element exhibits relatively good soft magnetic properties such as magnetic permeability and magnetic flux density. Therefore, for example, when molded into a magnetic core, a resin molding material that can exhibit good magnetic properties can be obtained.
[0043] As the form of the above-mentioned metal-containing material, in addition to the single substance, for example, there can be mentioned alloys such as solid solution, eutectic, and intermetallic compound, etc. By using particles composed of such a metal material, a resin molding material having excellent magnetic properties derived from iron, that is, high magnetic permeability and high magnetic flux density, etc. can be obtained.
[0044] Furthermore, the metal-containing material may contain elements other than iron as constituent elements. Examples of elements other than iron include B, C, N, O, Al, Si, P, S, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Cd, In, Sn, etc., and one of these or a combination of two or more of these may be used. In the present embodiment, one or more elements selected from Fe, Ni, Si, and Co may be contained as main elements.
[0045] Specific examples of the metal-containing material include pure iron, silicon steel, iron-cobalt alloy, iron-nickel alloy, iron-chromium alloy, iron-aluminum alloy, carbonyl iron, stainless steel, or composite materials containing one or more of these. Silicon steel and carbonyl iron can be preferably used from the viewpoint of availability.
[0046] The soft magnetic particles (Fe-based soft magnetic particles) may be particles other than these. For example, they may be magnetic particles containing Ni-based soft magnetic particles, Co-based soft magnetic particles, and the like.
[0047] Volume-based median particle size D of soft magnetic particles (A) 50 It is preferably 0.5 to 75 μm, more preferably 0.75 to 65 μm, and even more preferably 1 to 60 μm. By appropriately adjusting the particle size (median particle size), the flowability during molding can be further improved, and the magnetic properties can be enhanced.
[0048] In addition, D 50 For example, it can be obtained by a laser diffraction / scattering particle size distribution measuring device. Specifically, the particle size distribution curve can be obtained by measuring the soft magnetic particles (A) under dry conditions using a particle size distribution measuring device "LA-950" manufactured by HORIBA, and D can be obtained by analyzing the distribution curve. 50 .
[0049] The resin molding material of this embodiment contains the soft magnetic particles (A) in an amount of 96% by mass or more. The upper limit is 98% by mass or less. This can obtain a magnetic material with high magnetic permeability.
[0050] Furthermore, the resin molding material of the present embodiment contains the soft magnetic particles (A) in an amount of 82% by volume or more, preferably 84% by volume or more. The upper limit is 90% by volume or less.
[0051] [Organosilicon compound (B)]
[0052] As the organosilicon compound (B), known organosilicon compounds can be used within the scope of achieving the effects of the present invention. The organosilicon compound (B) is preferably liquid at room temperature (25° C.), thereby improving the fluidity of the resin molding material, thereby improving the filling property into the mold, and improving the wettability, and further suppressing the generation of voids, etc.
[0053] Patent document 1 (International Publication No. 2019 / 229960) states that by containing a siloxane compound, the overall elasticity of the composite can be reduced, thereby reducing the stress acting on the composite accompanying the molding shrinkage (thermosetting) of the composite (paragraph 0110). That is, it is believed that in this document, by using a solid siloxane compound in the case of melt kneading, a soft domain structure such as a micro-dispersed structure can be formed, thereby alleviating the stress of the composite after curing. On the other hand, in the present invention, by using an organosilicon compound (B) that is liquid at room temperature (25°C), the fluidity of the resin molding material (resin composition) during molding and the filling property into the mold can be improved, thereby improving the wettability, and thus the purpose is not to improve the physical properties of the cured molded product as in Patent Document 1.
[0054] As the organosilicon compound (B), an organosilicon compound represented by the following general formula (1) can be preferably used.
[0055]
[0056] In the general formula (1), R each independently represents a substituted or unsubstituted monovalent organic group having 1 to 10 carbon atoms, at least one of R is a group selected from an amino-substituted organic group, an epoxy-substituted organic group, an organic group containing a polyoxyalkylene group, a hydroxyl-substituted organic group, a vinyl-substituted organic group, a carboxyl-substituted organic group, an isocyanate-substituted organic group, a mercapto-substituted organic group, a (meth)acrylic acid-substituted organic group and an acid anhydride-substituted organic group. n represents an integer of 1 to 100.
[0057] When at least one of R is the above group, the remaining R is preferably an alkyl group or alkoxy group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, and further preferably an alkyl group having 1 to 5 carbon atoms.
[0058] In the present embodiment, from the viewpoint of the effects of the present invention, it is preferred that at least one of R is an epoxy-substituted organic group.
[0059] From the viewpoint of the effects of the present invention, the functional group equivalent of the organosilicon compound (B) is preferably 200 to 30,000, more preferably 300 to 20,000.
[0060] Furthermore, the weight average molecular weight of the organosilicon compound (B) is preferably 200 to 10,000, more preferably 500 to 8,000.
[0061] As the organosilicon compound (B), an organosilicon compound represented by the following general formula (1a) is preferably used.
[0062]
[0063] In the general formula (1a), Q is an epoxy-substituted organic group or a polyoxyalkylene-containing organic group, and a plurality of Qs may be the same or different. It is preferred that Q contains an epoxy-substituted organic group.
[0064] a represents an integer of 1 to 50, and b represents an integer of 1 to 50.
[0065] The epoxy-substituted organic group can be represented by the following general formula (a).
[0066]
[0067] In formula (a), X 1 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and the alkylene group may contain an ether group. * represents a bond.
[0068] The polyoxyalkylene group-containing organic group can be represented by the following general formula (b).
[0069]
[0070] In formula (b), X 2 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and R 1 It represents a hydrogen atom or an alkylene group having 1 to 3 carbon atoms.
[0071] c represents an integer of 1 to 20, and d represents an integer of 1 to 20.
[0072] * indicates a bond.
[0073] Examples of the organosilicon compound (B) include SF8421EG, FZ-3730, BY16-869, BY16-870, X-22-4741, X-22-178SX, and X-22-178DX (all manufactured by Dow Corning Toray Co., Ltd.), KF-1002, and X-22-343 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0074] From the viewpoint of the effect of the present invention, the resin molding material of the present embodiment may contain an organosilicon compound (B) in an amount preferably of 0.5% by mass or less, more preferably of 0.4% by mass or less, and further preferably of 0.3% by mass or less. The lower limit is 0.01% by mass or more, preferably 0.05% by mass or more. If the content of the organosilicon compound (B) exceeds this range, it may solidify at room temperature, resulting in reduced operability, especially uneven dispersion during compression molding, and sometimes the desired molded body may not be obtained.
[0075] In the present embodiment, the organosilicon compound (B) is not added for the purpose of improving the mold shrinkage, and the amount added is preferably within the above range.
[0076] The resin molding material of this embodiment contains the above-mentioned amount of soft magnetic particles (A) and the above-mentioned amount of fine powder silica (F), so that a magnetic material having high magnetic permeability can be obtained, and a resin molding material having sufficient fluidity and excellent filling properties into a mold can be obtained.
[0077] [Thermosetting resin (C)]
[0078] Thermosetting resin (C) can include, for example, epoxy resin, phenolic resin, polyimide resin, bismaleimide resin, urea-formaldehyde (urea) resin, melamine resin, polyurethane resin, cyanate resin, silicone resin, oxetane resin (oxetane compound), (methyl) acrylate resin, unsaturated polyester resin, diallyl phthalate resin, benzoxazine resin, etc. These can be used alone or in combination of two or more. From the viewpoint of heat resistance, the thermosetting resin (C) preferably contains an epoxy resin, for example.
[0079] The epoxy resin is not particularly limited as long as the effects of the present invention can be exhibited, and a known compound can be used.
[0080] (Epoxy resin)
[0081] Examples of the epoxy resin include bisphenol-A epoxy resin, bisphenol-F epoxy resin, tetramethylbisphenol-F epoxy resin, bisphenol-S epoxy resin, bisphenol-E epoxy resin, bisphenol-M epoxy resin, bisphenol-P epoxy resin, bisphenol-Z epoxy resin and the like; novolac-type epoxy resins such as phenol novolac-type epoxy resin and cresol novolac-type epoxy resin; biphenyl-type epoxy resin, biphenyl aralkyl-type epoxy resin, aryl alkylene-type epoxy resin, naphthalene-type epoxy resin, anthracene-type epoxy resin, phenoxy-type epoxy resin, dicyclopentadiene-type epoxy resin, norbornene-type epoxy resin, adamantane-type epoxy resin, fluorene-type epoxy resin, triphenylmethane-type epoxy resin and the like.
[0082] The resin molding material of the present embodiment may contain one epoxy resin or two or more epoxy resins, and may be of the same type or epoxy resins of different molecular weights.
[0083] From the viewpoint of the effects of the present invention, the epoxy resin of the present embodiment is preferably at least one selected from the group consisting of an epoxy resin containing a triphenylmethane structure, an epoxy resin containing a biphenyl structure, and a bisphenol A type or F type epoxy resin.
[0084] In the present embodiment, it is more preferable to use a combination of an epoxy resin containing a triphenylmethane structure and a bisphenol A type or F type epoxy resin, or an epoxy resin containing a biphenyl structure.
[0085] Specifically, the epoxy resin containing a triphenylmethane structure refers to an epoxy resin containing a partial structure in which three of the four hydrogen atoms of methane (CH4) are replaced by a benzene ring. The benzene ring may be unsubstituted or substituted with a substituent. Examples of the substituent include a hydroxyl group or a glycidoxy group.
[0086] Specifically, the epoxy resin containing a triphenylmethane structure contains a structural unit represented by the following general formula (a1): Two or more of these structural units are linked to form a triphenylmethane skeleton.
[0087]
[0088] In the general formula (a1),
[0089] R 11 When there are plural of them, they are each independently a monovalent organic group, a halogen atom, a hydroxyl group or a cyano group,
[0090] R 12 When there are plural of them, they are each independently a monovalent organic group, a halogen atom, a hydroxyl group or a cyano group,
[0091] i is an integer from 0 to 3,
[0092] j is an integer from 0 to 4.
[0093] As R 11 and R 12 Examples of the monovalent organic group include R in the general formula (BP) described below. a and R b The groups listed are monovalent organic groups.
[0094] i and j are each independently preferably 0-2, more preferably 0-1.
[0095] In one embodiment, both i and j are 0. That is, in one embodiment, all benzene rings in the general formula (a1) do not have a substituent other than the explicitly stated glycidoxy group as a monovalent substituent.
[0096] Specifically, the epoxy resin containing a biphenyl structure refers to an epoxy resin containing a structure in which two benzene rings are linked by a single bond. The benzene ring here may or may not have a substituent.
[0097] Specifically, the epoxy resin containing a biphenyl structure has a partial structure represented by the following general formula (BP).
[0098]
[0099] In the general formula (BP),
[0100] R a and R b When there are plural of them, they are each independently a monovalent organic group, a hydroxyl group or a halogen atom,
[0101] r and s are independently 0 to 4,
[0102] *Indicates connection with other atomic groups.
[0103] As R a and R b Specific examples of the monovalent organic group include an alkyl group, an alkenyl group, an alkynyl group, an alkylidene group, an aryl group, an aralkyl group, an alkaryl group, a cycloalkyl group, an alkoxy group, a heterocyclic group, and a carboxyl group.
[0104] Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl and decyl.
[0105] Examples of the alkenyl group include an allyl group, a pentenyl group, and a vinyl group.
[0106] Examples of the alkynyl group include ethynyl group and the like.
[0107] Examples of the alkylidene group include a methylene group and an ethylidene group.
[0108] Examples of the aryl group include tolyl, xylyl, phenyl, naphthyl and anthracenyl.
[0109] Examples of the aralkyl group include benzyl and phenethyl groups.
[0110] Examples of the alkaryl group include tolyl and xylyl groups.
[0111] Examples of the cycloalkyl group include adamantyl, cyclopentyl, cyclohexyl, and cyclooctyl.
[0112] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a sec-butoxy group, an isobutoxy group, a tert-butoxy group, an n-pentoxy group, a neopentoxy group, and an n-hexyloxy group.
[0113] Examples of the heterocyclic group include an epoxy group and an oxetanyl group.
[0114] R a and R b The total number of carbon atoms of the monovalent organic groups is, for example, 1 to 30, preferably 1 to 20, more preferably 1 to 10, particularly preferably 1 to 6.
[0115] r and s are each independently preferably 0 to 2, and more preferably 0 to 1. In one embodiment, both r and s are 0.
[0116] More specifically, the biphenyl structure-containing epoxy resin is preferably a biphenyl aralkyl type epoxy resin having a structural unit represented by the following general formula (BP1).
[0117]
[0118] In the general formula (BP1),
[0119] R a and R b The definition and specific method are the same as those of the general formula (BP),
[0120] The definitions and preferred ranges of r and s are the same as those of the general formula (BP),
[0121] R c When there are plural of them, they are each independently a monovalent organic group, a hydroxyl group or a halogen atom,
[0122] t is an integer from 0 to 3.
[0123] As R cSpecific examples of the monovalent organic group include a and R b The same groups as those listed in the specific examples of .
[0124] t is preferably 0-2, more preferably 0-1.
[0125] Specifically, examples of the bisphenol A type or F type epoxy resin (epoxy resin produced by a condensation reaction of bisphenol A or bisphenol F and epichlorohydrin) include epoxy resins represented by the following general formula (EP).
[0126]
[0127] In the general formula (EP),
[0128] A plurality of R's are independently a hydrogen atom or a methyl group, preferably a methyl group,
[0129] R a , R b , R c and R d When there are two or more of them, they are each independently a monovalent organic group, a hydroxyl group or a halogen atom,
[0130] p, q, r and s are each independently 0 to 4, preferably 0 to 2,
[0131] n is an integer of 0 or more, usually 0-10, preferably 0-5.
[0132] As R a , R b , R c and R d Specific examples of the monovalent organic group include the following: a and R b The same groups as those listed in the specific examples of the monovalent organic group.
[0133] In this embodiment, it is preferable to use a bisphenol A type epoxy resin in which R is a methyl group.
[0134] The amount of the epoxy resin in the resin molding material of the present embodiment is, for example, 0.1 to 20 mass %, or preferably 0.5 to 10 mass %.
[0135] The amount of the epoxy resin in the resin molding material of the present embodiment is, for example, 0.5 to 60% by volume, or preferably 3 to 40% by volume.
[0136] (Phenolic resin)
[0137] The phenolic resin is not particularly limited, and examples thereof include novolac-type phenolic resins and resol-type phenolic resins such as phenol novolac resins, cresol novolac resins, and bisphenol A novolac resins. Of these, one may be used alone or two or more may be used in combination.
[0138] Among the phenolic resins, phenol novolac resins are preferred.
[0139] (Urea-formaldehyde resin)
[0140] The urea-formaldehyde resin is not particularly limited, and examples thereof include resins obtained by condensation of urea and formaldehyde.
[0141] (Melamine resin)
[0142] The melamine resin is not particularly limited, and for example, a melamine resin obtained by reacting melamine and formaldehyde under a neutral or weak base condition can be used.
[0143] Furthermore, as the melamine resin, a commercially available melamine resin such as a melamine resin manufactured by Sumitomo Chemical Co., Ltd. may be used.
[0144] (Unsaturated polyester resin)
[0145] The unsaturated polyester resin is not particularly limited, and examples thereof include the most common orthophthalic type using phthalic anhydride as a raw material, isophthalic type using isophthalic acid as a raw material, and terephthalic type using terephthalic acid as a raw material, and also includes prepolymers thereof. Among these, one kind may be used alone or two or more kinds may be used in combination.
[0146] (Polyimide resin)
[0147] The polyimide resin is not particularly limited, and can be synthesized, for example, by copolymerizing a diamine, a dianhydride, and anhydride to synthesize a polyamic acid which is a precursor of a polyimide, and then imidizing the polyamic acid.
[0148] [Phenol curing agent (D)]
[0149] The resin molding material of the present embodiment may further contain a phenolic curing agent (D).
[0150] This can be expected to further improve the durability of the obtained molded product. Typically, the phenol-based curing agent has two or more hydroxyl groups in one molecule.
[0151] The phenolic curing agent preferably contains any one of a novolac skeleton and a biphenyl skeleton. When the phenolic curing agent contains any one of these skeletons, the durability of the molded body can be particularly improved.
[0152] Specifically, the "biphenyl skeleton" refers to a structure in which two benzene rings are linked by a single bond, as in the general formula (BP) in the description of the epoxy resin above.
[0153] Specifically, examples of the phenolic curing agent having a biphenyl skeleton include those having a structure in which the glycidyl group in the general formula (BP1) in the above description of the epoxy resin is substituted with a hydrogen atom.
[0154] Specifically, examples of the phenolic curing agent having a novolac skeleton include those having a structural unit represented by the following general formula (N).
[0155]
[0156] In the general formula (N),
[0157] R 4 represents a monovalent substituent,
[0158] u is an integer from 0 to 3.
[0159] As R 4 Specific examples of the monovalent substituents include the following: a and R b The same substances as described above with respect to the monovalent substituent.
[0160] u is preferably 0 to 2, more preferably 0 to 1, and even more preferably 0.
[0161] In the present embodiment, the phenolic curing agent (D) is preferably at least one selected from novolac-type phenolic resins and biphenyl aralkyl-type phenolic resins.
[0162] When the phenolic curing agent (D) is a polymer or an oligomer, the number average molecular weight (standard polystyrene conversion value based on GPC measurement) of the phenolic curing agent (D) is, for example, about 200 to 800.
[0163] The content of the phenolic curing agent (D) in the resin molding material is, for example, 0.1 to 20 mass %, or preferably 0.5 to 10 mass %.
[0164] The content of the phenolic curing agent (D) in the resin molding material is, for example, 0.5 to 60% by volume, or preferably 3 to 40% by volume.
[0165] By appropriately adjusting the amount of the phenolic curing agent (D), the fluidity can be further improved, and the mechanical properties and magnetic properties of the obtained cured product can be improved.
[0166] [Curing accelerator (E)]
[0167] The resin molding material of the present embodiment may further contain a curing accelerator (E). The curing accelerator (E) is not particularly limited as long as it can accelerate the curing reaction of the epoxy resin, and a known epoxy curing accelerator can be used.
[0168] Specifically, there can be mentioned: phosphorus-containing compounds such as organic phosphines, tetrasubstituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, adducts of phosphonium compounds and silane compounds; imidazoles (imidazole-based curing accelerators) such as 2-methylimidazole and 2-phenylimidazole; nitrogen-containing compounds such as amidines or tertiary amines, quaternary salts of amidines or amines, such as 1,8-diazabicyclo[5.4.0]undec-7-ene and benzyldimethylamine.
[0169] Preferred are tetrasubstituted phosphonium compounds, phosphobetaine compounds, phosphine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds.
[0170] When using a curing accelerator (E), only one kind may be used, or two or more kinds may be used.
[0171] When a curing accelerator (E) is used, its content is preferably 0.01 to 1% by mass, more preferably 0.04 to 0.8% by mass, relative to the entire resin molding material. The volume fraction is preferably 0.05 to 5% by volume, more preferably 0.10 to 0.4% by volume. By setting it to such a numerical range, a sufficient curing acceleration effect can be obtained without excessively deteriorating other properties.
[0172] [Fine powder silicon dioxide (F)]
[0173] The resin molding material of the present embodiment may further contain fine powder silica (F).
[0174] The average particle size of the fine powder silicon dioxide (F) is 0.1 μm to 2.0 μm, preferably 0.1 μm to 1.5 μm, and more preferably 0.1 μm to 1.0 μm. Thus, the fine powder silicon dioxide (F) can be uniformly dispersed in the resin molding material, so that the fluidity is further improved, thereby further improving the filling property and moldability, so that a molded body with less molding defects can be obtained, and particularly good magnetic properties can be obtained in the molded body.
[0175] The fine powder silica (F) has a high affinity with thermosetting resins and high insulating properties, and is therefore useful as a constituent material of non-magnetic powder for resin molding materials.
[0176] The true specific gravity of the fine powder silica (F) is preferably 1.0 to 6.0, more preferably 1.2 to 5.0, and further preferably 1.5 to 4.5. Such fine powder silica (F) has a small specific gravity and is therefore easy to flow with the melt of the thermosetting resin. Therefore, during molding, when the melt of the thermosetting resin flows toward the gap of the molding die, the fine powder silica (F) is easy to flow with the melt.
[0177] The sphericity of the fine powder silica (F) is not particularly limited, but is preferably 0.50 to 1.00, more preferably 0.75 to 1.00. When the sphericity of the fine powder silica (F) is within this range, the fluidity of the resin molding material can be ensured by the rolling of the fine powder silica (F) itself.
[0178] The resin molding material of this embodiment may contain 1.5 mass % or less, preferably 1.2 mass % or less, and more preferably 1.0 mass % or less of fine powder silicon dioxide (F). From the viewpoint of the effect of the present invention, the lower limit is 0.05 mass % or more, preferably 0.1 mass % or more.
[0179] Furthermore, the volume fraction of fine powder silicon dioxide (F) is 4 volume % or less, preferably 3 volume % or less, and more preferably 2 volume % or less. The lower limit is 0.14 volume % or more, and preferably 0.5 volume % or more.
[0180] The average particle size of the fine powder silica (F) refers to the volume average particle size (e.g., D 50 ), which can be measured using a laser diffraction particle size distribution measuring device.
[0181] In addition, when a perfect circle with the same area as that of each particle in a scanning electron microscope (SEM) image is regarded as an equal-area circle, the sphericity of particles such as fine powder silica (F) can be obtained by the equal-area circle equivalent diameter / circumscribed circle diameter. In addition, the equal-area circle equivalent diameter / circumscribed circle diameter is calculated for 10 or more particles selected at random, and the average value is taken as the "sphericity of the particle".
[0182] (Carboxylic acid dispersant)
[0183] The resin molding material of the present embodiment may further contain a carboxylic acid-based dispersant. By containing a carboxylic acid-based dispersant, the filling property of the resin molding material into the mold can be further improved.
[0184] As the carboxylic acid-based dispersant, any conventionally known compound can be used without particular limitation as long as the effects of the present invention can be exhibited. In the present embodiment, the carboxylic acid-based dispersant preferably contains at least one compound represented by the following general formula (i).
[0185]
[0186] In the general formula (i), R represents a carboxyl group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylcarboxyl group having 1 to 5 carbon atoms, an alkoxycarboxyl group having 1 to 5 carbon atoms, an alkyl alcohol group having 1 to 5 carbon atoms, or an alkoxyalcohol group having 1 to 5 carbon atoms, and multiple R groups may be the same or different.
[0187] R is preferably a carboxyl group, a hydroxyl group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkylcarboxyl group having 1 to 5 carbon atoms.
[0188] X represents an oxygen atom, an alkylene group having 1 to 30 carbon atoms, a divalent chain hydrocarbon group having 1 to 30 carbon atoms and having one or more double bonds, or a divalent chain hydrocarbon group having 1 to 30 carbon atoms and having one or more triple bonds, and a plurality of Xs may be the same or different. Examples of the divalent chain hydrocarbon group include an alkylene group and the like.
[0189] X is preferably an oxygen atom, an alkylene group having 1 to 20 carbon atoms, or a divalent chain hydrocarbon group having 1 to 20 carbon atoms and having one or more double bonds, and more preferably an oxygen atom, an alkylene group having 1 to 20 carbon atoms, or an alkylene group having 1 to 20 carbon atoms and having one or more double bonds.
[0190] n represents an integer of 0-20, and m represents an integer of 1-5.
[0191] The compound represented by the general formula (i) is preferably a compound represented by the following general formula (ia) or general formula (ib). The carboxylic acid-based dispersant may contain at least one selected from these.
[0192]
[0193] In the general formula (ia), R, m and n have the same meanings as in the general formula (i).
[0194]
[0195] In the general formula (ib), Q represents an alkylene group having 1 to 5 carbon atoms, preferably an alkylene group having 1 to 3 carbon atoms. X has the same meaning as in the general formula (1).
[0196] The acid value of the carboxylic acid dispersant is 5 to 500 mgKOH / g, preferably 10 to 350 mgKOH / g, and more preferably 15 to 100 mgKOH / g. When the acid value is within the above range, a magnetic material having a high saturation magnetic flux density and excellent fluidity and moldability can be obtained.
[0197] The carboxylic acid-based dispersant is preferably in a solid or waxy state.
[0198] From the viewpoint of the effects of the present invention, the content of the carboxylic acid-based dispersant is 0.01% by mass to 2% by mass, and preferably 0.05% by mass to 1% by mass, based on 100% by mass of the resin molding material.
[0199] Examples of the compound represented by the general formula (i) contained in the carboxylic acid-based dispersant include Hypermer KD-4 (mass average molecular weight: 1700, acid value: 33 mgKOH / g), Hypermer KD-9 (mass average molecular weight: 760, acid value: 74 mgKOH / g), Hypermer KD-12 (mass average molecular weight: 490, acid value: 111 mgKOH / g), and Hypermer KD-16 (mass average molecular weight: 370, acid value: 299 mgKOH / g) manufactured by CRODA.
[0200] (Other ingredients)
[0201] The resin molding material of this embodiment may contain components other than the above components, for example, one or more of a low stress agent, a coupling agent, an adhesion promoter, a mold release agent, a colorant, an antioxidant, a corrosion inhibitor, a dye, a pigment, a flame retardant, and the like.
[0202] Examples of the low stress agent include polybutadiene compounds, acrylonitrile butadiene copolymer compounds, silicone oils, silicone rubbers and other organic silicon compounds. When using a low stress agent, only one type may be used, or two or more types may be used in combination.
[0203] As the coupling agent, the coupling agent used for the surface treatment of magnetic particles can be used. For example, silane coupling agents, titanium coupling agents, zirconium oxide coupling agents, aluminum coupling agents, etc. can be cited. When using a coupling agent, only one type can be used, or two or more types can be used in combination.
[0204] Industrially, the resin molding material of the present embodiment can be manufactured, for example, by the following steps: first (1) using a mixer to mix the components, (2) then using a roller to knead the components at about 120° C. for more than 5 minutes, preferably about 10 minutes to obtain a kneaded product, (3) and then cooling the obtained kneaded product, (4) then further pulverizing it. Through the above steps, a powdered resin molding material can be obtained. The powdered resin molding material of the present embodiment suppresses agglomeration and consolidation, so it has excellent fluidity and improved operability.
[0205] (Form of resin molding material)
[0206] The resin molding material of this embodiment is preferably in the form of an ingot or a granule at 23° C., and more preferably in the form of an ingot. The powdered resin molding material can be ingoted to form an ingot. When the resin molding material is in the form of an ingot or a granule, it is easy to circulate or store the resin molding material, and it is easy to apply to transfer molding or compression molding.
[0207] The powdery resin molding material of the present embodiment suppresses aggregation and solidification, and can be formed into a tablet-shaped or granular composition having a uniform composition.
[0208] (Characteristics when melting resin molding material)
[0209] The resin molding material of the present embodiment contains a predetermined amount of the organosilicon compound (B), and thus the fluidity of the resin molding material when melted can be improved, and the filling property, moldability, and the like can be enhanced.
[0210] The filling property of the resin molding material can be confirmed with high accuracy by the following "expansion test" to determine the filling property and moldability of the resin molding material when it is melted. That is, by using the expansibility test to continuously apply stress to the entire molten resin molding material, the characteristics of the molten material melting and expanding can be confirmed, and the filling property and moldability into the mold can be confirmed with higher accuracy under conditions close to the actual manufacturing process. Due to the excellent characteristics of the resin molding material, the filling property and moldability into the details of the mold can be confirmed with high accuracy during injection molding, especially when the material is placed in the mold for heating / pressing during compression molding, the filling property and moldability into the mold can be confirmed with high accuracy.
[0211] (Extended test)
[0212] A spoonful (2.0 ml) of the resin molding material was placed on a gel plate at 175°C. A thin burr measurement mold (lower mold 3,000 g) heated to 175°C was placed on it and left for 5 minutes. The thin burr measurement mold was removed and the diameter of the resin molding material that was pressed into a roughly circular shape was measured.
[0213] Specifically, the flow length measured by the spiral flow test at a temperature of 175° C. can be set to 30 cm or more, preferably 40 cm or more, and more preferably 45 cm or more.
[0214] The spiral flow test can be conducted, for example, by using a low pressure transfer molding machine ("KTS-15" manufactured by KOHTAKI Corporation) under the conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a holding time of 180 seconds, injecting the resin molding material into a mold for spiral flow measurement based on EMMI-1-66 to measure the flow length.
[0215] Furthermore, the resin molding material of the present embodiment can have a Koka type viscosity measured using a Koka type viscosity measuring device under the conditions of a measuring temperature of 175°C and a load of 40 kgf of 30 Pa·s to 300 Pa·s, preferably 50 Pa·s to 250 Pa·s, and further preferably 60 Pa·s to 200 Pa·s.
[0216] (Glass transition temperature of cured product)
[0217] The glass transition temperature of the cured product obtained by post-curing the resin molding material of the present embodiment at 175°C for 4 hours in the atmosphere at 175°C is preferably 150 to 220°C, more preferably 160 to 200°C. By designing the resin molding material to have a glass transition temperature of 150°C or more, it is easy to achieve the heat resistance required for, for example, vehicle-mounted applications. By designing the resin molding material to have a glass transition temperature of 220°C or less, molding can be performed at a relatively low temperature. This is preferred from the viewpoint of suppressing the shrinkage of the molded product by low-temperature processing.
[0218] <Molding body>
[0219] The molded body of the present embodiment can be obtained by solidifying the above-mentioned resin molding material. In the powdered resin molding material of the present embodiment, although the filling amount of the soft magnetic particles (A) is high, due to the excellent filling property and moldability, the obtained molded body (magnetic material) has a uniform composition and can exert the desired characteristics in terms of magnetic properties such as magnetic permeability or saturation magnetic flux density or mechanical strength.
[0220] Specifically, the relative magnetic permeability of the molded article of the present embodiment is 40 or more, preferably 42 or more, and more preferably 45 or more.
[0221] Furthermore, as described above, the molded body of this embodiment is composed of a composite material having a uniform composition and a high saturation magnetic flux density, and thus can achieve a high saturation magnetic flux density of 1.0 T or more, preferably 1.2 T or more, and more preferably 1.3 T or more.
[0222] The method for producing the molded body is not particularly limited, and examples thereof include transfer molding and compression molding.
[0223] (Transfer molding)
[0224] The method for producing a molded body by transfer molding includes: injecting a melt of the resin molding material into a mold using a transfer molding device; solidifying the melt; and releasing the molded body from the mold.
[0225] Transfer molding can be performed by appropriately using a known transfer molding device or the like. Specifically, first, a preheated resin molding material is placed in a heating chamber, also called a transfer chamber, and melted to obtain a molten material. Thereafter, the molten material is injected into a mold using a push rod, and the molten material is held as it is to solidify. In this way, a desired molded product can be obtained.
[0226] Transfer molding is preferred in terms of improving the controllability of the size of the molded product and the degree of freedom in shape.
[0227] Various conditions in transfer molding can be set arbitrarily. For example, the preheating temperature can be appropriately adjusted between 60 and 100°C, the heating temperature during melting can be appropriately adjusted between 100 and 250°C, the mold temperature can be appropriately adjusted between 100 and 200°C, and the pressure when the molten resin molding material is injected into the mold can be appropriately adjusted between 1 and 20 MPa.
[0228] By not making the mold temperature too high, shrinkage of the molded product can be suppressed.
[0229] (Compression molding method)
[0230] The method for producing a molded body by compression molding includes the step of compression molding the resin molding material. Specifically, the method includes: the step of compression molding the resin molding material of the present embodiment in a mold; and the step of removing the molded body from the mold.
[0231] Compression molding can be performed using a known compression molding device. Specifically, the resin molding material is placed in a concave portion of a concave fixed mold that opens upward. The resin molding material can be preheated. Thus, the molded body can be uniformly solidified and the molding pressure can be reduced.
[0232] Next, the convex mold is moved from above to the concave fixed mold, and the resin molding material is compressed in the cavity formed by the convex part and the concave part. First, the resin molding material is fully softened and flowed under low pressure, and then the mold is closed and re-pressurized to solidify for a specified time.
[0233] Various conditions in compression molding can be set arbitrarily. For example, the preheating temperature can be appropriately adjusted between 60 and 100°C, the heating temperature during melting can be appropriately adjusted between 100 and 250°C, the mold temperature can be appropriately adjusted between 100 and 200°C, the pressure when the resin molding material is compressed by the mold can be appropriately adjusted between 1 and 20 MPa, and the curing time can be appropriately adjusted between 60 and 300 seconds.
[0234] By not making the mold temperature too high, shrinkage of the molded product can be suppressed.
[0235] The resin molding material of this embodiment can obtain a magnetic material having high magnetic permeability. Therefore, a molded body obtained by curing the resin molding material can be used for a magnetic core in an inductor or an outer casing member that seals a magnetic core and a coil.
[0236] use Figure 1 The outline of a structure (integrated inductor) including an outer packaging member formed of a cured product of the resin molding material according to the present embodiment will be described.
[0237] Figure 1 (a) shows the outline of the structure 100 as viewed from the upper surface. Figure 1 (b) means Figure 1 (a) is a cross-sectional view observed along the AA' cross section.
[0238] like Figure 1 As shown, the structure 100 of the present embodiment may include a coil 10 and a magnetic core 20. The magnetic core 20 is filled inside the coil 10 (air-core coil). The coil 10 and the magnetic core 20 are sealed by an outer packaging member 30 (sealing member). The magnetic core 20 and the outer packaging member 30 may be formed of a cured product of the resin molding material of the present embodiment. The magnetic core 20 and the outer packaging member 30 may be formed as a seamless integral member.
[0239] As a method for manufacturing the structure 100 of the present embodiment, for example, the coil 10 may be arranged in a mold, and the resin molding material of the present embodiment may be used, and the resin molding material may be solidified by mold molding such as transfer molding, thereby forming an outer packaging member 30 integrally with the magnetic core 20 filled in the coil 10 and the surroundings thereof. At this time, the coil 10 may have a lead-out portion (not shown) for leading the end of the winding wire to the outside of the outer packaging member 30.
[0240] The coil 10 is generally composed of a winding structure in which a metal wire surface is wound with an insulating coating. The metal wire is preferably a highly conductive metal wire, and copper or a copper alloy can be appropriately used. In addition, the insulating coating can be coated with enamel or the like. The cross-sectional shape of the winding wire can be circular, rectangular, hexagonal, etc.
[0241] On the other hand, the cross-sectional shape of the core 20 is not particularly limited, and may be circular, quadrilateral, hexagonal, or other polygonal shape when viewed in cross section. The core 20 is formed of a transfer molded product of the resin molding material of this embodiment, and thus may have a desired shape.
[0242] According to the cured product of the resin molding material of this embodiment, the magnetic core 20 and the outer packaging component 30 having excellent magnetic properties such as moldability and high magnetic permeability can be realized, so the structure 100 (integrated inductor) having these can be expected to have low magnetic loss. In addition, the outer packaging component 30 having excellent mechanical properties can be realized, so the durability, reliability and manufacturing stability of the structure 100 can be improved. Therefore, the structure 100 of this embodiment can be used for an inductor for a boost circuit or a large current.
[0243] As mentioned above, although the embodiment of this invention was described, these are only examples of this invention, and various structures other than the above-mentioned can be adopted within the range which does not impair the effect of this invention.
[0244] Example
[0245] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited thereto.
[0246] <Examples 1 to 5, Comparative Examples 1 and 2>
[0247] First, the components listed in Table 1 were prepared at the listed ratios, and the soft magnetic particles were mixed first, and then the other components were added thereto and mixed uniformly to obtain a mixture.
[0248] Next, the obtained mixture was kneaded at 120°C for 10 minutes. After the kneading was completed, the obtained kneaded material was cooled to room temperature to make it solid, and then pulverized and tablet-shaped. Through the above steps, a tablet-shaped resin molding material was obtained.
[0249] The following shows the raw material components described in Table 1. The following shows the evaluation results of the resin molding materials and molded products in Table 1. In addition, the content (volume %) of the soft magnetic particles described in Table 1 is the content (i.e., filling rate) when the resin molding material containing the soft magnetic particles is 100 volume %.
[0250] (Soft magnetic particles)
[0251] Iron-based particles 1: amorphous magnetic powder (manufactured by EPSON ATMIX Corporation, KUAMET6B2, median particle size D 50 :50μm)
[0252] Iron-based particles 2: amorphous magnetic powder (manufactured by EPSON ATMIX Corporation, AW2-08, median particle size D 50 :4μm)
[0253] (Micronized Silica)
[0254] Micronized silica 1: fused silica, median particle size D50 =0.5μm
[0255] (Epoxy resin)
[0256] Epoxy resin 1: jER1032H60: an epoxy resin containing a triphenylmethane structure manufactured by Mitsubishi Chemical Corporation, which is solid at 23° C. and contains the structural unit represented by the above general formula (a1).
[0257] Epoxy resin 2: YL-6810: A bisphenol A epoxy resin manufactured by Mitsubishi Chemical Corporation, which is solid at 23° C. and has a structure represented by the above general formula (EP).
[0258] Epoxy resin 3: NC3000L: a biphenyl aralkyl type epoxy resin manufactured by Nippon Kayaku Co., Ltd., which is solid at 23° C. and contains the structural unit represented by the above general formula (BP1).
[0259] (Curing agent)
[0260] Curing agent 1: PR-HF-3: a novolac-type phenolic resin manufactured by Sumitomo Bakelite Co., Ltd., which is solid at 23°C.
[0261] Curing agent 2: MEH-7851SS: a phenol aralkyl resin containing a biphenylene skeleton manufactured by Meiwa Chemicals Co., Ltd., which is solid at 23°C.
[0262] (Adhesion aid)
[0263] Adhesion aid 1: CDA-1M (heavy metal deactivator, made by ADEKA CORPORATION)
[0264] (Release Agent)
[0265] Release agent 1: WE-4 (wax, manufactured by Clariant Chemicals Ltd.)
[0266] (catalyst)
[0267] Catalyst 1: A compound represented by the following chemical formula.
[0268]
[0269] 37.5 g (0.15 mol) of 4,4'-bisphenol S and 100 ml of methanol were placed in a separable flask with a stirring device, stirred and dissolved at room temperature, and then a solution obtained by dissolving 4.0 g (0.1 mol) of sodium hydroxide in 50 ml of methanol was added while stirring. Next, a solution obtained by dissolving 41.9 g (0.1 mol) of tetraphenylphosphonium bromide in 150 ml of methanol was added. Stirring was continued for a while, and after adding 300 ml of methanol, the solution in the flask was added dropwise to a large amount of water while stirring to obtain a white precipitate. The precipitate was filtered and dried to obtain the above-mentioned catalyst 1 as white crystals.
[0270] Catalyst 2: A compound represented by the following chemical formula.
[0271]
[0272] 249.5 g of phenyltrimethoxysilane and 384.0 g of 2,3-dihydroxynaphthalene were added to a flask containing 1800 g of methanol to dissolve them, and then 231.5 g of a 28% sodium methoxide-methanol solution was added dropwise under stirring at room temperature. Furthermore, a solution prepared by dissolving 503.0 g of tetraphenylphosphonium bromide in 600 g of methanol was added dropwise under stirring at room temperature, resulting in the precipitation of crystals. The precipitated crystals were filtered, washed with water, and vacuum dried to obtain catalyst 2 in the form of peach white crystals.
[0273] (Coupling agent)
[0274] Coupling agent 1: CF-4083 (phenylaminopropyltrimethoxysilane, manufactured by Dow Corning Toray Co., Ltd.)
[0275] (Metal Dispersants)
[0276] Dispersant 1: Hypermer KD-9 (mass average molecular weight: 760, acid value: 74 mgKOH / g, manufactured by CRODA)
[0277] (Organic silicon compounds)
[0278] Silicone oil: Silicone oil represented by the following chemical formula (liquid at room temperature (25° C.), FZ-3730, manufactured by Dow Corning Toray Co., Ltd.)
[0279]
[0280] <Evaluation>
[0281] (Extended test)
[0282] A spoonful (2.0 ml) of the resin molding material was placed on a gel plate at 175°C. A thin burr measurement mold (lower mold 3,000 g) heated to 175°C was placed on it and left for 5 minutes. The thin burr measurement mold was removed and the diameter of the resin molding material that was pressed into a roughly circular shape was measured.
[0283] (Flowability: spiral flow test)
[0284] The spiral flow test was carried out using the resin molding materials of Examples and Comparative Examples.
[0285] The test was conducted by injecting the resin molding material into a mold for spiral flow measurement based on EMMI-1-66 using a low-pressure transfer molding machine (Kohtaki Precision Machine Co., Ltd. "KTS-15") at a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a holding time of 180 seconds to measure the flow length. The larger the value, the better the fluidity.
[0286] (High viscosity)
[0287] The high-pressure viscosity of the resin molding material was measured using a high-pressure viscosity measuring device (High-pressure flow tester, Shimadzu Corporation, CFT-100EX) under the conditions of a measuring temperature of 175° C., a load of 40 kgf, and a nozzle size of 1.0 mm in diameter×10 mm in length.
[0288] (Relative magnetic permeability)
[0289] The resin molding material was injection molded using a low-pressure transfer molding machine (KOHTAKI Corporation "KTS-30") at a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 120 seconds to obtain a disk-shaped molded product with a diameter of 50mmΦ and a thickness of 3mm. Then, the obtained molded product was post-cured at 175°C for 4 hours. After that, it was processed into a toroidal shape with an outer diameter of 27mmΦ and an inner diameter of 15mmΦ by a router, and a test piece for relative magnetic permeability evaluation was produced. A primary coil of 42 turns and a secondary coil of 42 turns were wound around the obtained toroidal molded product, and an AC measurement was performed using a DC-AC magnetization characteristic test device (Metron Giken Co., Ltd. "MTR-1488"). The value at a frequency of 50KHz and a magnetic flux density of 50mT was taken as the relative magnetic permeability.
[0290] [Table 1]
[0291]
[0292] As shown in Table 1, in the comparison between Comparative Example 1 and Examples 1 and 2, and Comparative Example 2 and Examples 3 to 5, the results of the expansion test of the resin molding material of the embodiment of the present invention are: the diameter is large, and the melting and expansion characteristics are excellent when stress is continuously applied to the entire molten resin molding material, from which it is inferred that the filling property and moldability in the mold are excellent. Furthermore, the filling amount of soft magnetic particles can be increased, so a magnetic material with high magnetic permeability is obtained.
[0293] This application claims priority based on Japanese Patent Application No. 2020-168308 filed on October 5, 2020, and all the contents disclosed therein are incorporated herein by reference.
[0294] Description of Reference Numerals
[0295] 100: structure; 10: coil; 20: magnetic core; 30: outer packaging component.
Claims
1. A resin molding material for transfer molding or compression molding, the resin molding material comprising: Soft magnetic particles having a coercive force of 800 A / m or less (A); An organosilicon compound (B) which is liquid at room temperature of 25°C; Thermosetting resin (C); and Phenolic curing agent (D), The content of the soft magnetic particles (A) is 96% by mass or more, The organosilicon compound (B) is represented by the following general formula (1a): Thermosetting resin (C) is epoxy resin, The epoxy resin is at least one selected from bisphenol A epoxy resin, tris(hydroxyphenyl)methane epoxy resin and biphenyl aralkyl epoxy resin. The phenolic curing agent (D) is at least one selected from novolac type phenolic resin and biphenyl aralkyl type phenolic resin, In the general formula (1a), Q is an epoxy-substituted organic group represented by the following general formula (a) or a polyoxyalkylene-containing organic group represented by the following general formula (b), and a plurality of Qs present may be the same or different, a represents an integer of 1 to 50, and b represents an integer of 1 to 50. In formula (a), X 1 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and the alkylene group may contain an ether group, and * represents a bonding bond, *--X 2 -(C 2 H 4 O) c -(C 3 H 6 O) d -R 1 (b) In formula (b), X 2 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and R 1 represents a hydrogen atom or an alkylene group having 1 to 3 carbon atoms, c represents an integer of 1 to 20, d represents an integer of 1 to 20, and * represents a bond.
2. The resin molding material according to claim 1, Features: The content of the organosilicon compound (B) is 0.5% by mass or less.
3. The resin molding material according to claim 1 or 2, Features: It also contains a curing accelerator (E), The curing accelerator (E) is selected from tetrasubstituted phosphonium compounds, phosphate betaine compounds, phosphine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds.
4. The resin molding material according to claim 1 or 2, Features: The material further contains fine powder silicon dioxide (F) having an average particle size of 0.1 μm or more and 2.0 μm or less.
5. The resin molding material according to claim 1 or 2, Features: It is in the form of tablets or granules at 23°C.
6. The resin molding material according to claim 1 or 2, Features: The spiral flow length measured by the EMMI-1-66 method under the conditions of a mold temperature of 175° C., an injection pressure of 6.9 MPa, and a holding time of 180 seconds is 30 cm or more.
7. The resin molding material according to claim 1 or 2, Features: The high-pressure viscosity measured by using a high-pressure viscosity measuring device under the conditions of a measurement temperature of 175° C. and a load of 40 kgf is 30 Pa·s or more and 300 Pa·s or less.
8. A shaped body, Features: The resin molding material is obtained by curing the resin molding material according to any one of claims 1 to 7.
9. The molded article according to claim 8, Features: The relative magnetic permeability is 40 or more.
10. A method for producing a molded body, It is characterized in that include: A step of injecting a melt of the resin molding material according to any one of claims 1 to 7 into a mold using a transfer molding device; and The step of solidifying the melt.
11. A method for producing a molded body, It is characterized in that include: A step of compression molding the resin molding material according to any one of claims 1 to 7.
12. A resin molding material for transfer molding or compression molding, wherein: include: Soft magnetic particles having a coercive force of 800 A / m or less (A); Organosilicon compound (B); Thermosetting resin (C); and Phenolic curing agent (D), The content of the soft magnetic particles (A) is 96% by mass or more, The organosilicon compound (B) is represented by the following general formula (1a): The content of the organosilicon compound (B) is 0.5% by mass or less, Thermosetting resin (C) is epoxy resin, The epoxy resin is at least one selected from bisphenol A epoxy resin, tris(hydroxyphenyl)methane epoxy resin and biphenyl aralkyl epoxy resin. The phenolic curing agent (D) is at least one selected from novolac type phenolic resin and biphenyl aralkyl type phenolic resin, In the general formula (1a), Q is an epoxy-substituted organic group represented by the following general formula (a) or a polyoxyalkylene-containing organic group represented by the following general formula (b), and a plurality of Qs present may be the same or different, a represents an integer of 1 to 50, and b represents an integer of 1 to 50. In formula (a), X 1 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and the alkylene group may contain an ether group, and * represents a bonding bond, *--X 2 -(C 2 H 4 O) c -(C 3 H 6 O) d -R 1 (b) In formula (b), X 2 represents an alkylene group having 1 to 10 carbon atoms or an oxyalkylene group having 1 to 10 carbon atoms, and R 1 represents a hydrogen atom or an alkylene group having 1 to 3 carbon atoms, c represents an integer of 1 to 20, d represents an integer of 1 to 20, and * represents a bond.