Inorganic adsorption material and preparation method and use thereof

By reacting sodium carbonate, zirconium oxychloride and sodium dihydrogen phosphate under stirring conditions, inorganic adsorption materials were prepared, and the safety and efficiency problems of high-temperature and high-pressure preparation methods were solved, and materials with porous structure and good biocompatibility were obtained. Its application range and improves adsorption effect.

CN116328711BActive Publication Date: 2024-11-12JIAXING GAOZHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310062540.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-13
Publication Date
2024-11-12
Estimated Expiration
2043-01-13

AI Technical Summary

Technical Problem

The existing preparation method of sodium zirconium phosphate requires high temperature and high pressure, which poses safety hazards and difficulty in mixing reaction raw materials. The synthesis time is long, which limits its industrial production and application.

Method used

Sodium carbonate, zirconium oxychloride and sodium dihydrogen phosphate are used to react under stirring conditions, and inorganic adsorbed materials are obtained by adjusting the reaction conditions, avoiding high-pressure reactions, simplifying the process flow, and improving synthesis efficiency.

Benefits of technology

The prepared inorganic adsorbent materials have porous structures and good biocompatibility, which expands their application fields, and significantly improves their adsorption and ion exchange capabilities. They are suitable for support, photoelectric, catalysis and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116328711B_ABST
    Figure CN116328711B_ABST
Patent Text Reader

Abstract

The present invention provides an inorganic adsorption material and a preparation method and application thereof, the method comprising the following steps: 1) mixing sodium carbonate, zirconium oxychloride and water, reacting to obtain a mixed system; 2) adding sodium dihydrogen phosphate to the mixed system of step 1), reacting to prepare the inorganic adsorption material. The inorganic adsorption material has a porous structure, and the inorganic adsorption material can adsorb more metal ions by adsorption and ion exchange, thereby achieving a better adsorption effect. Moreover, the inorganic adsorption material and the antibacterial agent are prepared by aqueous solution, and compared with the prior art, the preparation method is more environmentally friendly and safer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adsorption materials, and in particular relates to an inorganic adsorption material and a preparation method and application thereof. Background Art

[0002] In today's increasingly polluted environment, the application and development of environmentally friendly and green adsorption materials are highly valued. Sodium zirconium phosphate has a special structure, which is a layered structure formed by the common point connection of PO4 tetrahedron and ZrO6 octahedron, and further forms a three-dimensional network structure with holes. The cations in the network can be replaced by other ions, so that sodium zirconium phosphate has ion exchange and adsorption capabilities. It is currently widely used in the fields of medicine, carriers, optoelectronics, catalysis, etc.

[0003] At present, the commonly used preparation method of sodium zirconium phosphate is hydrothermal synthesis under high temperature and high pressure, that is, a high-pressure reactor needs to be used during the reaction process, which is not conducive to industrial scale-up production from a safety perspective; in addition, there are defects such as difficulty in mixing the reaction raw materials and long synthesis time. Summary of the invention

[0004] In order to improve the deficiencies of the prior art, the present invention provides an inorganic adsorption material and a preparation method and use thereof. The preparation process of the inorganic adsorption material is simple, no high-pressure reactor is required, and the reaction raw materials are easy to mix during the reaction, and it has the advantages of short synthesis time and green environmental protection. The inorganic adsorption material prepared by the method has both adsorption and biocompatibility, which greatly expands the application field and scope of application of the inorganic adsorption material.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] A method for preparing an inorganic adsorption material, the method comprising the following steps:

[0007] 1) mixing sodium carbonate, zirconium oxychloride and water, reacting to obtain a mixed system;

[0008] 2) adding sodium dihydrogen phosphate to the mixed system of step 1) to react and prepare the inorganic adsorption material.

[0009] According to an embodiment of the present invention, in step 1), the mass ratio of sodium carbonate to zirconium oxychloride is 1:3-10, for example, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.

[0010] According to an embodiment of the present invention, in step 1), the mass ratio of zirconium oxychloride to water is 1:1-3, for example, 1:1, 1:1.2, 1:1.25, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.5, 1:2.8 or 1:3.

[0011] According to an embodiment of the present invention, in step 1), the reaction is carried out under stirring conditions, and the stirring speed is, for example, 100 to 300 rpm.

[0012] According to an embodiment of the present invention, in step 1), the reaction temperature is 70°C to 100°C (for example, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C), and the reaction time is, for example, 1 to 4 hours (for example, 1 hour, 2 hours, 3 hours or 4 hours).

[0013] According to an embodiment of the present invention, in step 1), preferably, zirconium oxychloride is first dissolved in water, and then sodium carbonate is added to the aqueous solution of zirconium oxychloride, mixed, and reacted to obtain a mixed system.

[0014] According to an embodiment of the present invention, in step 1), the mixed system after the reaction includes sodium zirconium carbonate.

[0015] According to an embodiment of the present invention, in step 2), the molar mass ratio of the sodium dihydrogen phosphate and the zirconium oxychloride is (0.2-1) mol:100g, that is, (0.2-1) mol of sodium dihydrogen phosphate is added to 100g of zirconium oxychloride, for example, 0.2 mol:100g, 0.3 mol:100g, 0.4 mol:100g, 0.5 mol:100g, 0.6 mol:100g, 0.7 mol:100g, 0.8 mol:100g, 0.9 mol:100g or 1 mol:100g.

[0016] According to an embodiment of the present invention, in step 2), the pH value of the reaction system is 2 to 4. The pH value of the reaction system can be adjusted by adding sodium dihydrogen phosphate.

[0017] According to an embodiment of the present invention, in step 2), the reaction temperature is 70°C to 100°C (for example, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C) and the reaction time is, for example, 1 to 12 hours (for example, 1 hour, 2 hours, 3 hours, 4 hours, 6 hours, 8 hours, 10 hours or 12 hours).

[0018] According to an embodiment of the present invention, in step 2), the reaction is carried out under stirring conditions, and the stirring speed is, for example, 100 to 300 rpm.

[0019] According to an embodiment of the present invention, in step 2), the inorganic adsorption material obtained after the reaction is sodium zirconium phosphate.

[0020] According to an embodiment of the present invention, the method further comprises the following steps:

[0021] 3) post-treating the reaction product of step 2).

[0022] According to an embodiment of the present invention, in step 3), the post-treatment includes at least one of filtration, washing and drying. Exemplarily, the post-treatment includes filtration, washing and drying.

[0023] According to an embodiment of the present invention, the washing is performed 3 to 10 times, the drying temperature is 60 to 100° C., and the drying time is 6 to 24 hours.

[0024] The present invention also provides an inorganic adsorption material prepared by the method.

[0025] According to an embodiment of the present invention, the inorganic adsorption material is sodium zirconium phosphate.

[0026] According to an embodiment of the present invention, the inorganic adsorption material has a porous structure.

[0027] According to an embodiment of the present invention, the surface of the inorganic adsorption material has a coral-like or honeycomb-like porous structure.

[0028] According to an embodiment of the present invention, the pore size of the inorganic adsorption material is nanometer scale.

[0029] According to an embodiment of the present invention, the pore size distribution of the inorganic adsorption material is 10nm to 100nm; exemplarily, the pore size distribution of the inorganic adsorption material is 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm or any point value in the range composed of the above two end point values.

[0030] According to an embodiment of the present invention, the particle size distribution of the inorganic adsorption material is in the micro-nano level, preferably in the micron level.

[0031] According to an embodiment of the present invention, the particle size distribution of the inorganic adsorbent material is 0.2μm to 200μm; exemplarily, the particle size distribution of the inorganic adsorbent material is 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 2μm, 3μm, 5μm, 8μm, 10μm, 20μm, 30μm, 50μm, 80μm, 90μm, 100μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm or any point value in the range composed of the above two end point values.

[0032] According to an embodiment of the present invention, the cation absorption capacity of the inorganic adsorption material is ≥ 0.5 mmol / g. The cation is, for example, a metal ion, such as silver ion and / or copper ion.

[0033] The present invention also provides the use of the inorganic adsorption material, which is used in the fields of carrier, adsorption, photoelectricity and catalytic reaction.

[0034] According to an embodiment of the present invention, the inorganic adsorption material is used as an antibacterial agent, to purify dialysate, to adsorb heavy metals, to load cations or dye compounds with fluorescent properties to prepare photoelectric materials, and the like.

[0035] The present invention also provides an antibacterial agent, which comprises the above-mentioned inorganic adsorption material.

[0036] According to an embodiment of the present invention, the antibacterial agent further includes metal ions.

[0037] According to an embodiment of the present invention, the mass of the metal ions accounts for 1 to 10 wt% of the total mass of the antibacterial agent, for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%.

[0038] According to an embodiment of the present invention, the antibacterial agent is prepared by mixing the above-mentioned inorganic adsorption material with metal ions.

[0039] According to an embodiment of the present invention, the metal ions are selected from one or both of silver ions and copper ions.

[0040] The present invention also provides a method for preparing the above antibacterial agent, the method comprising the following steps:

[0041] The inorganic adsorption material of the present invention is mixed with a solution containing metal ions, and the mixed solution is heated to prepare the antibacterial agent.

[0042] According to an embodiment of the present invention, the heating temperature is 70-100° C., and the heating time is, for example, 1-6 hours.

[0043] According to an embodiment of the present invention, stirring is performed while the mixed liquid is heated, and the stirring speed is, for example, 100 to 300 rpm.

[0044] According to an embodiment of the present invention, the method comprises the following steps:

[0045] The inorganic adsorption material is suspended in water, and a solution containing metal ions is added dropwise while stirring. After the addition is completed, the mixed solution is heated and stirred. After the reaction is completed, the mixed solution is filtered and dried to prepare the antibacterial agent.

[0046] According to an embodiment of the present invention, the concentration of metal ions in the solution containing metal ions is 1 to 10 wt %.

[0047] According to an embodiment of the present invention, the solution containing metal ions is, for example, one or both of a silver nitrate aqueous solution and a copper nitrate aqueous solution.

[0048] According to an embodiment of the present invention, the drying temperature is, for example, 60 to 100° C., and the drying time is, for example, 12 to 48 hours.

[0049] The present invention also provides the use of the antibacterial agent, which is used for antibacterial coatings, antibacterial PVDF membranes, and the like.

[0050] Beneficial effects of the present invention:

[0051] The present invention provides an inorganic adsorption material and a preparation method and application thereof. The method of the present invention does not require reaction under high pressure and uses water as a solvent, so it is more environmentally friendly and safer than the prior art. Sodium carbonate is used in the reaction to obtain particles that are more evenly dispersed. The inorganic adsorption material prepared by the present invention has a porous structure, and the surface has a coral-like or honeycomb-like porous structure, which can adsorb more metal ions through adsorption and ion exchange, thereby achieving a better adsorption effect. When the inorganic adsorption material is used in an antibacterial agent, it can have very good antibacterial activity. For example, an antibacterial agent with a silver ion content of more than 3% in the inorganic adsorption material can have an antibacterial rate of more than 98%. . BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 SEM image of the inorganic adsorption material prepared in Example 1 of the present invention.

[0053] Figure 2 SEM image of the inorganic adsorption material prepared in Example 1 of the present invention.

[0054] Figure 3SEM image of the inorganic adsorption material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0055] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0056] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0057] Example 1

[0058] Dissolve 400g of zirconium oxychloride in 500ml of water, add 50g of sodium carbonate to the aqueous solution of zirconium oxychloride, stir and heat to 100°C, react for 1 hour, then add 600ml of 2M sodium dihydrogen phosphate solution, adjust the pH to 3, stir and heat to 100°C, react for 1 hour, filter, wash with water 3 times, dry in a forced air drying oven, dry at 80°C for 24 hours, sieve to obtain an inorganic adsorption material with a porous structure.

[0059] Figure 1 , Figure 2 and Figure 3 The SEM images at different magnifications of the inorganic adsorption material prepared in Example 1 are shown. As can be seen from the figure, the surface of the inorganic adsorption material has a coral-like porous structure with a pore size of nanometers; the particle size distribution of the inorganic adsorption material is micrometers.

[0060] Example 2

[0061] Take 63g of the inorganic adsorption material powder with a particle size of 300 mesh prepared in Example 1, add water and 0.1M AgNO3 solution, stir at 250rpm, heat to 70℃ and keep constant temperature for 3 hours, then filter when the temperature drops to 30℃, put the filter cake into an evaporating dish, place it in a blast drying oven and dry it at 80℃ for 24 hours. The amount of each material is shown in the following table:

[0062]

[0063] Sample 1, sample 2 and sample 3 were mixed into PVDF powder to make PVDF membrane 1, PVDF membrane 2 and PVDF membrane 3 respectively, and blank PVDF membrane was prepared at the same time, and then the antibacterial ability was tested. The test basis is: GBT31402-2015 Test method for antibacterial performance of plastic surface. The tested bacteria are: Escherichia coli and Staphylococcus aureus. Sample pretreatment: Place the PVDF membrane to be tested under ultraviolet light for 5 minutes. The test results are as follows:

[0064]

[0065]

[0066] Among them, the viable E. coli count of the PVDF membrane blank at 0h was 9.0×10 3 (CFU / ml). The viable count of Staphylococcus aureus obtained by testing the blank PVDF membrane at 0h was 1.6×10 4 (CFU / ml).

[0067] It can be seen that the inorganic adsorption material of the present invention can introduce silver ions into the inorganic adsorption material by adsorption and ion exchange. When the content of silver ions in the inorganic adsorption material is more than 3%, the antibacterial rate is higher than 98%, and as the silver ion content increases, the antibacterial ability is stronger.

[0068] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an inorganic adsorption material, wherein: The method comprises the following steps: 1) mixing sodium carbonate, zirconium oxychloride and water, reacting to obtain a mixed system; 2) adding sodium dihydrogen phosphate to the mixed system of step 1) to react and prepare the inorganic adsorption material; The inorganic adsorption material is sodium zirconium phosphate; The surface of the inorganic adsorption material has a coral-like or honeycomb-like porous structure; In step 1), the mixed system after the reaction includes sodium zirconium carbonate; In step 2), the pH value of the reaction system is 2 to 4; In step 2), the reaction temperature is 70-100°C.

2. The method for preparing an inorganic adsorption material according to claim 1, wherein: In step 1), the mass ratio of sodium carbonate to zirconium oxychloride is 1:3-10.

3. The method for preparing an inorganic adsorption material according to claim 1, wherein: In step 1), the mass ratio of zirconium oxychloride to water is 1:1-3.

4. The method for preparing an inorganic adsorption material according to claim 1, wherein: In step 1), the reaction temperature is 70-100° C., and the reaction time is 1-4 hours.

5. The method for preparing an inorganic adsorption material according to claim 1, wherein: In step 2), the molar mass ratio of the sodium dihydrogen phosphate and zirconium oxychloride is (0.2-1) mol:100g.

6. The method for preparing an inorganic adsorption material according to claim 1, wherein: In step 2), the reaction time is 1 to 12 hours.

7. The inorganic adsorption material prepared by the method according to any one of claims 1 to 6.

8. The inorganic adsorbent material according to claim 7, wherein: The pore size of the inorganic adsorption material is nanometer level.

9. The inorganic adsorbent material according to claim 7, wherein: The pore size distribution of the inorganic adsorption material is 10nm to 100nm.

10. The inorganic adsorbent material according to claim 7, wherein: The particle size distribution of the inorganic adsorption material is micro-nano level.

11. The inorganic adsorbent material according to claim 7, wherein: The particle size distribution of the inorganic adsorption material is 0.2 μm to 200 μm.

12. Use of the inorganic adsorption material according to any one of claims 7 to 11, in the fields of carrier, adsorption, photoelectricity and catalytic reaction.

13. An antibacterial agent, wherein The antibacterial agent comprises the inorganic adsorption material according to any one of claims 7 to 11.

14. The antibacterial agent according to claim 13, wherein The antimicrobial agent also includes metal ions.

15. The antibacterial agent according to claim 14, wherein The mass of the metal ions accounts for 1 to 10 wt % of the total mass of the antibacterial agent.

16. The antibacterial agent according to claim 14, wherein The antibacterial agent is prepared by exchanging the inorganic adsorption material with metal ions.

17. The antibacterial agent according to claim 14, wherein The metal ions are selected from one or both of silver ions and copper ions.

18. A method for preparing the antibacterial agent according to any one of claims 13 to 17, comprising the following steps: The inorganic adsorption material is mixed with a solution containing metal ions to carry out an ion exchange reaction to prepare the antibacterial agent.

19. The antibacterial agent according to claim 18, wherein The temperature of the ion exchange reaction is 70 to 100° C., and the time of the ion exchange reaction is 1 to 6 hours.

20. Use of the antibacterial agent according to any one of claims 13 to 17, which is used in antibacterial coatings and antibacterial PVDF membranes.