A hydrocracking catalyst and its preparation method
By using hierarchical pore SAPO-34 molecular sieve in the hydrocracking catalyst to provide a rich pore structure, it solves the problems of small pores and low selectivity of existing catalysts, and achieves efficient aviation fuel yield and quality improvement.
Patent Information
- Application Number
- CN202111590606.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-23
AI Technical Summary
The acidic component of existing hydrocracking catalysts is mainly provided by Y-type molecular sieves. The pore structure is small, making it difficult for the catalyst to perform optimally. The selectivity to jet fuel is not high, and there are problems such as temperature rise during the reaction cycle.
Multi-stage pore SAPO-34 molecular sieve is used as the acidic component to provide abundant micropore-mesoporous-macroporous channels, which improves the conversion, mass and heat transfer of wax oil macromolecule reactants, and improves the yield and quality of aviation fuel. . The catalyst includes a carrier and active metal. The carrier is composed of hierarchical porous SAPO-34, amorphous silica-alumina, modified Y molecular sieve and alumina, and is prepared through a specific mixing and roasting process.
In the wax oil hydrocracking reaction, the yield and quality of jet fuel are improved, ensuring high jet fuel yield and the generation of high-quality jet fuel, and solving the problems of pore structure limitations and insufficient selectivity of existing catalysts.
Smart Images

Figure BDA0003429800720000101 
Figure BDA0003429800720000111
Abstract
Description
Technical Field
[0001] The invention relates to a hydrocracking catalyst for producing more aviation kerosene and a preparation method thereof. The hydrocracking catalyst comprises a multi-level pore SAPO-34 molecular sieve. Background Art
[0002] Hydrocracking technology is one of the important means of deep processing of heavy oil. It has many advantages such as strong raw material adaptability, flexible processing scheme, high liquid product yield, and good product quality. Jet fuel has high quality and is a high-quality raw material for high-quality aviation fuel. It can be directly used as military aviation fuel. The by-product heavy naphtha has a high potential content of aromatics and is a high-quality raw material for catalytic chemical production of aromatics or high-octane gasoline. At the same time, it can also produce clean diesel blending components that meet the National VI standard. Hydrocracking technology has gradually developed into a key secondary processing technology for modern refining and chemical companies to produce clean oil products and high-quality chemical raw materials.
[0003] The hydrocracking catalyst consists of two parts: a carrier and an active component. The main function of the carrier is to provide a place for the metal active component to disperse. At the same time, the carrier itself provides suitable acidity during the catalytic reaction and completes the entire reaction together with the active component. The hydrogenation component of the hydrocracking catalyst is provided by metal oxides selected from Group VIII and Group VIB in the periodic table, while the acidic component is mainly provided by molecular sieves and inorganic oxides.
[0004] However, the acidic components of the hydrocracking catalyst prepared by the existing method are mostly borne by Y-type molecular sieves, which have a small pore structure and a single size. The prepared catalyst is difficult to exert its optimal performance, and there are also a series of problems such as low selectivity for the target product and high temperature rise in the reaction cycle.
[0005] WO2020119754A1 discloses a hydrocracking catalyst and its preparation method and application. The catalyst in the patent includes a carrier, silica loaded on the carrier and an active component. The carrier contains Y molecular sieve and SAPO-34 molecular sieve. The catalyst prepared by this method can improve the yield of jet fuel, but the cost of silane in the synthetic material is relatively high.
[0006] CN105536855A discloses a method for preparing a hydrocracking catalyst containing a Y molecular sieve, wherein the Y molecular sieve, amorphous silicon aluminum and / or alumina are used as carriers, and an active metal-containing carrier is used to obtain a hydrocracking catalyst. The hydrocracking catalyst prepared by this method has good temperature sensitivity and operational flexibility, but the pores of the Y molecular sieve are relatively single.
[0007] CN106140282B provides a method for preparing a hydrocracking catalyst of a composite molecular sieve, wherein the relative crystallinity of the β molecular sieve after steam hydrothermal treatment is above 95%, and the catalyst has high activity and medium oil selectivity, but the catalyst has low jet fuel selectivity.
[0008] CN105709844A discloses a hydrocracking catalyst carrier and a preparation method thereof. The catalyst carrier adopts a modified Y-type molecular sieve and a β molecular sieve as a cracking center, wherein the Y-type molecular sieve used is a Y-type molecular sieve with large grains, high silicon and concentrated effective pore size distribution. The hydrocracking catalyst prepared from the Y-type molecular sieve is used in the hydrocracking process of producing more high-quality intermediate distillate oil products, and has the characteristics of high activity and good selectivity, but the catalyst has low selectivity for aviation kerosene.
[0009] CN104667969B The invention discloses a hydrocracking catalyst and a preparation method thereof. The catalyst comprises a β molecular sieve, a Y-type molecular sieve and an alumina carrier. The hydrocracking catalyst has the characteristics of suitable silicon-aluminum ratio, large specific surface area, suitable acidity, reasonable pore structure and low non-framework aluminum content. The prepared catalyst can be used to produce more low-freezing point diesel and improve the properties of chemical raw materials, but the catalyst has low aviation kerosene selectivity. Summary of the invention
[0010] The core acidic molecular sieve used in the hydrocracking catalyst is a microporous molecular sieve, which will limit the diffusion and heat transfer of macromolecular reactants. Based on this feature, the hydrocracking catalyst of the present invention contains a certain proportion of multi-level channel SAPO-34 as a part of the acidic component, and provides relatively abundant micropore-mesopore-macroporous channels as reaction channels, which improves the conversion, mass transfer and heat transfer of macromolecular reactants and products of wax oil in the hydrocracking reaction of wax oil containing macromolecules, and can improve the yield and quality of aviation kerosene in the process of wax oil hydrocracking.
[0011] In view of the deficiencies of the prior art, the present invention discloses a hydrocracking catalyst and a preparation method thereof. The catalyst is characterized in that it contains multi-level pore SAPO-34 as a part of the acidic component, and provides relatively abundant micropore-mesopore-macroporous pores as reaction channels, which improves the conversion, mass transfer and heat transfer of wax oil macromolecular reactants and products in the hydrocracking reaction of wax oil containing macromolecules, and can improve the yield and quality of aviation kerosene in the process of wax oil hydrocracking. Using the hydrocracking crude oil of a refinery of PetroChina as the raw material, under a one-stage cascade reaction process, the application of this catalyst can ensure a higher jet kerosene yield and high-quality jet kerosene quality.
[0012] To achieve the above-mentioned purpose, the present invention provides a hydrocracking catalyst, which includes a carrier and an active metal, wherein the carrier includes a multi-level porous SAPO-34 molecular sieve, and the multi-level porous SAPO-34 includes a total amount of 8 to 25 wt% of chitosan oligosaccharides and soluble starch, based on the weight of the aluminum source.
[0013] Furthermore, the content of the carrier is 87-62 wt %, and the content of the active metal is 13-38 wt %.
[0014] Furthermore, the active metal is W and / or Ni; the active metal is calculated by weight of oxide, the oxide content of W is 10-30wt%, and the oxide content of Ni is 3-8wt%.
[0015] Furthermore, it also includes P, and the oxide content of P is 0.1-3wt% based on the weight of oxide.
[0016] Furthermore, the raw materials of the carrier include multi-level pore SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve and alumina.
[0017] Furthermore, based on the weight of the carrier, the content of the modified Y molecular sieve and the multi-level pore SAPO-34 molecular sieve is 5wt% to 35wt%, wherein the mass ratio of the modified Y molecular sieve to the multi-level pore SAPO-34 molecular sieve is 1:3 to 5:1; the content of amorphous silicon aluminum is 10wt% to 45wt%, and the content of aluminum oxide is 20wt% to 85wt%.
[0018] Furthermore, the silicon oxide content in the amorphous silicon aluminum is 19-58wt%.
[0019] Furthermore, the silicon-aluminum ratio of the modified Y molecular sieve is 7-30, and the unit cell parameter is 2.43-2.46 nm.
[0020] Furthermore, the preparation method of the carrier can be carried out by the following specific steps: adding an auxiliary agent to a mixture including multi-level porous SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve, and alumina, kneading, extruding wet strips, drying and calcining the wet strips to obtain the carrier.
[0021] Furthermore, the preparation method of the carrier can also be carried out by the following specific steps: first, the multi-level porous SAPO-34 molecular sieve and amorphous silica-alumina are mixed, and then a mixture including modified Y molecular sieve and alumina is added, and then an auxiliary agent is added, and the mixture is fully kneaded, and wet strips are extruded, and the wet strips are dried and calcined to obtain the carrier.
[0022] Furthermore, the preparation process of the carrier also includes adding methyl cellulose, and the amount of methyl cellulose used is 1% to 5wt% based on the weight of the carrier.
[0023] Furthermore, the auxiliary agent is an acidic solution prepared from water, nitric acid and citric acid.
[0024] Furthermore, the drying temperature is 70-120° C. and the drying time is 3-9 h.
[0025] Furthermore, the calcination temperature is 410-590° C. and the calcination time is 3-9 h.
[0026] Furthermore, based on the weight of the aluminum source, the amount of chitosan oligosaccharide added is 7-20wt%, and the amount of soluble starch added is 1-5wt%.
[0027] Preferably, the preparation method of the multi-level pore SAPO-34 molecular sieve specifically comprises the following steps:
[0028] (1) dissolving chitosan oligosaccharide in water to obtain a chitosan oligosaccharide solution;
[0029] (2) adding an aluminum source, a silicon source and a phosphorus source to the chitosan oligosaccharide solution of step (1), mixing evenly, and stirring to obtain a mixture;
[0030] (3) adding a template to the mixture of step (2), and then adding soluble starch, and then crystallizing to obtain a molecular sieve slurry containing multi-level pores;
[0031] (4) Filtering, drying and calcining the molecular sieve slurry obtained in step 3) to obtain a multi-level pore SAPO-34 molecular sieve.
[0032] Furthermore, in step (3), after adding the template, soluble starch is added under alkaline conditions.
[0033] Furthermore, the aluminum source is one or more of pseudo-boehmite, aluminum sulfate, aluminum chloride, and aluminum nitrate, preferably pseudo-boehmite.
[0034] Furthermore, the silicon source is one or more of active silicon dioxide, white carbon black, sodium silicate, ethyl orthosilicate, silica sol, water glass, and white carbon black, preferably water glass.
[0035] Furthermore, the template agent is one or more of diethylamine, triethylamine, morpholine, diisopropylamine, di-n-propylamine, diethanolamine, triethanolamine, tetraethylammonium hydroxide, and N,N-diethylethanol, preferably diethylamine.
[0036] Furthermore, the phosphorus source is phosphoric acid or metaphosphoric acid.
[0037] Furthermore, in step (1), the dissolution temperature is 10 to 100° C., preferably 30 to 70° C.; and the dissolution time is 0 to 280 min, preferably 10 to 160 min.
[0038] Furthermore, in step (3), the molar ratio of the aluminum source, phosphorus source, silicon source, template and water in the molecular sieve slurry is (1-3):(3-6):(0.5-2):(3-16):(100-360).
[0039] Furthermore, in step (3), the crystallization temperature is 40 to 400° C., preferably 50 to 280° C.; the crystallization time is 0 to 14400 min, preferably 10 to 4320 min.
[0040] Furthermore, in step (4), the drying temperature is 70-120° C., the drying time is 3-9 h, the roasting temperature is 410-590° C., and the roasting time is 3-9 h.
[0041] The present invention also provides a method for preparing a hydrocracking catalyst, the preparation method comprising:
[0042] The carrier is impregnated in an impregnation solution containing active metals, dried and calcined to obtain a hydrocracking catalyst; the impregnation process is to supersaturate the carrier with the W-Ni complex impregnation solution, and the active metals are based on the weight of the catalyst, with the oxide of W being 10-30%, the oxide of nickel being 3-8%, and the oxide of P being 0.1-3%.
[0043] Furthermore, the W-Ni complex impregnation solution is prepared by mixing a soluble active metal salt, phosphoric acid and a complexing agent and dissolving them in deionized water or ammonia water. The complexing agent is one or more of citric acid, ethanolamine, diethanolamine, triethanolamine, aminoacetic acid, ethylenediamine and ethylenediaminetetraacetic acid.
[0044] The hydrocracking catalyst of the present invention can be used to catalyze the hydrogenation reaction of straight-run wax oil and / or diesel raw materials, and is particularly suitable for the catalytic hydrogenation reaction of raw materials with dry point ≯550°C, residual carbon ≯0.3ω% and nitrogen content ≯1200μg / g.
[0045] The present invention has the following beneficial effects:
[0046] (1) The hydrocracking catalyst of the present invention improves the conversion, mass transfer and heat transfer of wax oil macromolecular reactants and products in the hydrocracking reaction of wax oil containing macromolecules.
[0047] (2) The hydrocracking catalyst of the present invention can improve the yield and quality of aviation kerosene during the hydrocracking process of wax oil. DETAILED DESCRIPTION
[0048] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments that do not specify specific conditions are usually based on conventional conditions. The wt% of the present invention represents mass percentage.
[0049] Evaluation and analysis methods: including BET determination, actual boiling point cut-off, and condensation point determination. The specific surface area and pore volume of the sample were determined using a Quantachrome autosorb-analyzer adsorption instrument. The jet fuel yield was determined using an i-fischer model DIST D-2892CC actual boiling point distillation instrument, and the condensation point data was determined using a BF-15 condensation point tester from Dalian North Analytical Instruments Co., Ltd.
[0050] Example 1
[0051] (1) Preparation of hierarchical pore SAPO-34 molecular sieve
[0052] Weigh 4.45g of chitosan oligosaccharide and add it to 100.02g of deionized water, and stir it thoroughly at 50°C for 16min; add 22.11g of pseudo-boehmite, 31.35g of phosphoric acid, and 11.69g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 19.62g of diethylamine and 141.10g of deionized water to the mixture, and then add 1.03g of water-soluble starch, and stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle with a polytetrafluoroethylene liner, place it in a 190°C oven for crystallization for 3696min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 5000r / min for 20min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 560°C for 6h to obtain a multi-level pore SAPO-34 molecular sieve A-1;
[0053] (2) Preparation of hydrocracking catalyst carrier
[0054] 12.0g of molecular sieve A-1, 60.8g of Y molecular sieve, 72.8g of alumina, 62.4g of amorphous silica-alumina and 6.5g of methyl cellulose were mixed and put into a kneader for 25 minutes. 124.3g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2mm for three times, and finally formed into a cylindrical strip with a diameter of 1.8mm. The obtained wet strip was dried in an oven at 111°C for 11h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain carrier B-1.
[0055] (3) Preparation of hydrocracking catalyst
[0056] At room temperature, dissolve 2.0g of citric acid, 19.5g of nickel nitrate hexahydrate, 5.0g of phosphoric acid (85wt%) and 33.0g of ammonium metatungstate in 30mL of deionized water in turn, make the impregnation solution dilute to 65mL, take 100g of carrier B-1 prepared in the previous step and place it in an impregnation tank, pour in the impregnation solution, soak for 4h, first cure the impregnated carrier in a 30℃ oven for 12h, then dry in a 120℃ oven for 8h, finally place it in a muffle furnace and heat to 520℃ and calcine for 4h to obtain catalyst C-1.
[0057] Example 2
[0058] (1) Preparation of hierarchical pore SAPO-34 molecular sieve
[0059] Weigh 3.13g of chitosan oligosaccharide and add it to 100.02g of deionized water, and stir it thoroughly at 60°C for 16min; add 16.31g of aluminum oxide, 31.35g of phosphoric acid, and 11.69g of water glass to the obtained solution, mix them evenly, and stir them for 1h; continue to add 19.62g of diethylamine and 141.10g of deionized water to the mixture, and then add 0.73g of water-soluble starch, and stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle with a polytetrafluoroethylene liner, place it in a 190°C oven for crystallization for 3666min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 5000r / min for 20min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 560°C for 6h to obtain a multi-level pore SAPO-34 molecular sieve A-2;
[0060] (2) Preparation of hydrocracking catalyst carrier
[0061] 15.6 g of molecular sieve A-1, 35.36 g of Y molecular sieve, 75.7 g of alumina, 81.32 g of amorphous silica-alumina and 6.5 g of methyl cellulose were mixed and put into a kneader for 25 minutes. 124.3 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 1.8 mm. The obtained wet strip was dried in an oven at 111°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain carrier B-2.
[0062] (3) Preparation of hydrocracking catalyst
[0063] At room temperature, dissolve 2.0g of citric acid, 19.5g of nickel nitrate hexahydrate, 5.0g of phosphoric acid (85wt%) and 33.0g of ammonium metatungstate in 30mL of deionized water in turn, make the impregnation solution dilute to 65mL, take 100g of carrier B-2 prepared in the previous step and place it in an impregnation tank, pour in the impregnation solution, soak for 4h, first cure the impregnated carrier in a 30℃ oven for 12h, then dry in a 120℃ oven for 8h, finally place it in a muffle furnace and heat to 520℃ and calcine for 4h to obtain catalyst C-2.
[0064] Example 3
[0065] (1) Preparation of hierarchical pore SAPO-34 molecular sieve
[0066] Weigh 2.46g of chitosan oligosaccharide and add it to 100.02g of deionized water, and stir it thoroughly at 50°C for 16min; add 22.11g of pseudo-boehmite, 31.35g of phosphoric acid, and 11.69g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 19.62g of diethylamine and 141.10g of deionized water to the mixture, and then add 0.80g of water-soluble starch, and stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle with a polytetrafluoroethylene liner, place it in a 190°C oven for crystallization for 3696min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 5000r / min for 20min, wash the crystals until the pH is less than 8, dry the crystals at 100°C, and then place the crystals in a muffle furnace and roast them at 560°C for 5.5h to obtain a multi-level pore SAPO-34 molecular sieve A-3;
[0067] (2) Preparation of hydrocracking catalyst carrier
[0068] 23.08g of molecular sieve A-1, 39.10g of Y molecular sieve, 55.14g of alumina, 90.68g of amorphous silica-alumina and 6.5g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 25 minutes. 124.3g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded three times through a cylindrical orifice plate with a diameter of 2mm, and finally formed into a cylindrical strip with a diameter of 1.8mm. The obtained wet strip was dried in an oven at 111°C for 11h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain carrier B-3.
[0069] (3) Preparation of hydrocracking catalyst
[0070] At room temperature, dissolve 2.0g of citric acid, 19.5g of nickel nitrate hexahydrate, 5.0g of phosphoric acid (85wt%) and 33.0g of ammonium metatungstate in 30mL of deionized water in turn, make the impregnation solution dilute to 65mL, take 100g of carrier B-3 prepared in the previous step and place it in an impregnation tank, pour in the impregnation solution, soak for 4h, first cure the impregnated carrier in a 30℃ oven for 12h, then dry in a 120℃ oven for 8h, finally place it in a muffle furnace and heat to 520℃ and calcine for 4h to obtain catalyst C-3.
[0071] Comparative Example 1
[0072] (1) Preparation of SAPO-34 molecular sieve
[0073] Weigh 0.00g of chitosan oligosaccharide and add it to 100.02g of deionized water, and stir it thoroughly at 50°C for 16min; add 22.11g of pseudo-boehmite, 31.35g of phosphoric acid, and 11.69g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 19.62g of diethylamine and 141.10g of deionized water to the mixture, and then add 0.00g of water-soluble starch, and stir them thoroughly to obtain a uniform gel mixture; transfer the gel mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 190°C oven for crystallization for 3696min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 5000r / min for 20min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and roast them at 560°C for 6h to obtain SAPO-34 molecular sieve A-4;
[0074] (2) Preparation of hydrocracking catalyst carrier
[0075] 12.0g of molecular sieve A-4, 60.8g of Y molecular sieve, 72.8g of alumina, 62.4g of amorphous silica-alumina and 6.5g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 25 minutes. 124.3g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2mm for three times, and finally formed into a cylindrical strip with a diameter of 1.8mm. The obtained wet strip was dried in an oven at 111°C for 12h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain carrier B-4.
[0076] (3) Preparation of hydrocracking catalyst
[0077] At room temperature, dissolve 2.0g of citric acid, 19.5g of nickel nitrate hexahydrate, 5.0g of phosphoric acid (85wt%) and 33.0g of ammonium metatungstate in 30mL of deionized water in turn, make the impregnation solution dilute to 65mL, take 100g of carrier B-1 prepared in the previous step and place it in an impregnation tank, pour in the impregnation solution, soak for 4h, first cure the impregnated carrier in a 30℃ oven for 12h, then dry in a 120℃ oven for 8h, finally place it in a muffle furnace and heat to 520℃ and calcine for 4h to obtain catalyst C-4.
[0078] Comparative Example 2
[0079] (1) Preparation of hydrocracking catalyst carrier
[0080] 15.6 g of molecular sieve A-4, 35.36 g of Y molecular sieve, 75.7 g of alumina, 81.32 g of amorphous silica-alumina and 6.5 g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 25 minutes. 124.3 g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2 mm for three times, and finally formed into a cylindrical strip with a diameter of 1.8 mm. The obtained wet strip was dried in an oven at 111°C for 12 hours, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4 hours to obtain carrier B-5.
[0081] (2) Preparation of hydrocracking catalyst
[0082] At room temperature, 2.0 g of citric acid, 19.5 g of nickel nitrate hexahydrate, 5.0 g of phosphoric acid (85 wt%) and 33.0 g of ammonium metatungstate were dissolved in 30 mL of deionized water in sequence. The impregnation solution was adjusted to 65 mL. 100 g of carrier B-2 prepared in the previous step was placed in an impregnation tank and the impregnation solution was poured in. After soaking for 4 hours, the impregnated carrier was cured in an oven at 30 ° C for 12 hours, and then dried in an oven at 120 ° C for 8 hours. Finally, it was placed in a muffle furnace and the temperature was raised to 520 ° C and calcined for 4 hours to obtain catalyst C-5.
[0083] Comparative Example 3
[0084] (1) Preparation of hydrocracking catalyst carrier
[0085] 23.08g of molecular sieve A-4, 39.10g of Y molecular sieve, 55.14g of alumina, 90.68g of amorphous silica-alumina and 6.5g of methyl cellulose were mixed and put into a kneader for mixing and grinding for 25 minutes. 124.3g of an acidic solution prepared by water, nitric acid and citric acid was added to the dry powder at one time. The mixture was first kneaded into a paste, and then extruded through a cylindrical orifice plate with a diameter of 2mm for three times, and finally formed into a cylindrical strip with a diameter of 1.8mm. The obtained wet strip was dried in an oven at 111°C for 12h, and finally placed in a muffle furnace and programmed to rise to 550°C and calcined for 4h to obtain carrier B-6.
[0086] (2) Preparation of hydrocracking catalyst
[0087] At room temperature, dissolve 2.0g of citric acid, 19.5g of nickel nitrate hexahydrate, 5.0g of phosphoric acid (85wt%) and 33.0g of ammonium metatungstate in 30mL of deionized water in turn, make the impregnation solution dilute to 65mL, take 100g of carrier B-3 prepared in the previous step and place it in an impregnation tank, pour in the impregnation solution, soak for 4h, first cure the impregnated carrier in a 30℃ oven for 12h, then dry in a 120℃ oven for 8h, finally place it in a muffle furnace and heat to 520℃ for calcination for 4h to obtain catalyst C-6.
[0088] Comparative Example 4:
[0089] Weigh 0.00g of chitosan oligosaccharide and add it to 50.12g of deionized water, and stir it thoroughly at 30°C for 16min; add 11.13g of pseudo-boehmite, 15.62g of phosphoric acid, and 5.72g of water glass to the obtained solution, mix well, and stir for 1h; continue to add 9.72g of diethylamine and 70.10g of deionized water to the solution, and then add 0.55g of water-soluble starch, and stir well to obtain a uniform mixture; transfer the gel-like mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 180°C oven for crystallization for 4056min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 2500r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 110°C, and then place the crystals in a muffle furnace and calcine them at 550°C for 6h to obtain SAPO-34 molecular sieve A-5.
[0090] Comparative Example 5:
[0091] Weigh 0.41g of chitosan oligosaccharide and add it to 50.12g of deionized water, and stir it thoroughly at 90°C for 16min; add 11.13g of pseudo-boehmite, 15.62g of phosphoric acid, and 5.73g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 30.72g of tetraethylammonium hydroxide and 70.10g of deionized water to the solution, and then add 0.34g of water-soluble starch, and stir them thoroughly to obtain a uniform mixture; transfer the gel-like mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 180°C oven for crystallization for 6021min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 2500r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 100°C, and then place the crystals in a muffle furnace and roast them at 520°C for 6h to obtain SAPO-34 molecular sieve A-6.
[0092] Comparative Example 6:
[0093] Weigh 4.38g of chitosan oligosaccharide and add it to 50.12g of deionized water, and stir it thoroughly at 60°C for 16min; add 11.13g of pseudo-boehmite, 15.62g of phosphoric acid, and 6.76g of silica sol to the obtained solution, mix them evenly, and stir them for 1h; continue to add 30.72g of tetraethylammonium hydroxide and 70.10g of deionized water to the solution, and then add 0.75g of water-soluble starch, and stir them thoroughly to obtain a uniform mixture; transfer the gel-like mixture to a stainless steel kettle containing a polytetrafluoroethylene liner, place it in a 182°C oven for crystallization for 6021min to obtain a crystallization solution; centrifuge the crystallization solution after crystallization at a speed of 2500r / min for 30min, wash the crystals until the pH is less than 8, dry the crystals at 100°C, and then place the crystals in a muffle furnace and roast them at 530°C for 4h to obtain SAPO-34 molecular sieve A-7.
[0094] The molecular sieves, supports and catalysts obtained in the examples and comparative examples were evaluated and analyzed, and the results are shown in Tables 1 to 3.
[0095] Table 1 Molecular sieve properties
[0096]
[0097]
[0098] Table 2 Carrier properties
[0099] project B-1 B-2 B-3 B-4 B-5 B-6 <![CDATA[Specific surface area, m 2 / g]]> 433 466 493 405 411 401 <![CDATA[Pore volume, cm 3 / g]]> 0.72 0.74 0.73 0.65 0.54 0.69 SAPO-34 molecular sieve, wt% 5.8 7.5 11.1 5.8 7.5 11.1 Y molecular sieve, wt% 29.2 17.0 18.8 15.1 17.0 18.8 Amorphous silicon aluminum, wt% 30.0 39.1 43.6 30.0 39.1 43.6 Alumina, wt% margin margin margin margin margin margin
[0100] Table 3 Catalyst properties
[0101] project C-1 C-2 C-3 C-4 C-5 C-6 <![CDATA[WO3,wt%]]> 21.6 21.6 21.6 21.6 21.6 21.6 NiO, wt% 5.0 5.0 5.0 5.0 5.0 5.0 <![CDATA[Specific surface area, m 2 / g]]> 223.5 235.7 227.5 199.8 211.5 208.7 Pore volume, mL / g 0.39 0.41 0.42 0.28 0.30 0.33
[0102] From the results in Table 1, it can be seen that the multi-level pore SAPO-34 molecular sieve synthesized by the present invention has a high specific surface area and contains abundant micro-meso-macropore channels, which is beneficial to the mass transfer and heat transfer of reactants.
[0103] It can be seen from the results in Table 2 that the carrier prepared by using the multi-level pore SAPO-34 molecular sieve synthesized by the present invention has the advantages of high specific surface area and pore volume.
[0104] From the results in Table 3, it can be seen that the catalyst prepared by using the multi-level pore SAPO-34 molecular sieve synthesized by the present invention has the advantages of high specific surface area and pore volume.
[0105] The hydrocracking catalysts prepared in the examples and comparative examples were subjected to activity evaluation tests. The test was conducted on a 200 mL pilot plant, using a one-stage series process, and the operating conditions were as follows: hydrogen partial pressure 15.0 MPa, hydrogen-to-oil volume ratio 1100:1, liquid hourly volume space velocity 1.6 h -1 , control the nitrogen content in the cracking section to be no more than 10ppm, and the product properties are shown in Table 4.
[0106] Table 4 Product properties
[0107] catalyst A-1 A-2 A-3 A-4 A-5 A-6 Jet fuel yield 52.25 48.56 53.35 42.57 39.39 41.37 Jet fuel freezing point -61.3 -59.5 -60.1 -49.3 -52.7 -55.1
[0108] It can be seen from the results in Table 4 that the catalyst of the present invention has excellent hydrocracking activity, high jet fuel selectivity and low jet fuel freezing point.
[0109] The above embodiments are typical examples listed to illustrate the technical solutions of the present invention in detail. The present invention is subject to the protection scope of the claims and the content of the invention and is not limited by the implementation scheme. Simple replacement or modification of the present invention is still within the protection scope of the present invention.
Claims
1. A hydrocracking catalyst, comprising a carrier and an active metal, wherein the carrier comprises a multi-level porous SAPO-34 molecular sieve, characterized in that: The preparation method of the multi-level pore SAPO-34 molecular sieve specifically comprises the following steps: (1) dissolving chitosan oligosaccharide in water to obtain a chitosan oligosaccharide solution; (2) adding an aluminum source, a silicon source and a phosphorus source to the chitosan oligosaccharide solution of step (1), mixing evenly, and stirring to obtain a mixture; (3) adding a template to the mixture of step (2), and then adding soluble starch to crystallize to obtain a molecular sieve slurry containing multi-level pores; (4) filtering, drying, and calcining the molecular sieve slurry obtained in step (3) to obtain a multi-level pore SAPO-34 molecular sieve; During the preparation of the multi-level pore SAPO-34 molecular sieve, chitosan oligosaccharide and soluble starch are added in a total amount of 8 to 25 wt % based on the weight of the aluminum source.
2. The hydrocracking catalyst according to claim 1, characterized in that The content of the carrier is 97-62wt%, and the content of the active metal is 3-38wt%.
3. The hydrocracking catalyst according to claim 1, characterized in that The active metal is W and / or Ni; the active metal is calculated by weight of oxide, the oxide content of W is 10-30wt%, and the oxide content of Ni is 3-8wt%.
4. The hydrocracking catalyst according to claim 1, characterized in that It also includes P, and the P oxide content is 0.1-3wt% based on the weight of the oxide.
5. The hydrocracking catalyst according to claim 1, characterized in that The raw materials of the carrier include multi-level pore SAPO-34 molecular sieve, amorphous silica-alumina, modified Y molecular sieve and alumina; based on the weight of the carrier, the content of the modified Y molecular sieve and the multi-level pore SAPO-34 molecular sieve is 5wt% to 35wt%, wherein the mass ratio of the modified Y molecular sieve to the multi-level pore SAPO-34 molecular sieve is 1:3 to 5:1; the content of amorphous silica-alumina is 10wt% to 45wt%, and the content of alumina is 20wt% to 85wt%.
6. The hydrocracking catalyst according to claim 5, characterized in that The silicon oxide content in the amorphous silicon aluminum is 19-58wt%; the silicon aluminum ratio of the modified Y molecular sieve is 7-30, and the unit cell parameter is 2.43-2.46nm.
7. The hydrocracking catalyst according to claim 1, characterized in that The added amount of the chitosan oligosaccharide is 7-20wt%, and the added amount of the soluble starch is 1-5wt%.
8. The hydrocracking catalyst according to claim 1, characterized in that In step (3), after adding the template, soluble starch is added under alkaline conditions; the aluminum source is one or more of pseudo-boehmite, aluminum sulfate, aluminum chloride, and aluminum nitrate; the silicon source is one or more of active silica, white carbon black, sodium silicate, tetraethyl orthosilicate, silica sol, water glass, and white carbon black; the template is one or more of diethylamine, triethylamine, morpholine, diisopropylamine, di-n-propylamine, diethanolamine, triethanolamine, tetraethylammonium hydroxide, and N,N-diethylethanolamine; and the phosphorus source is phosphoric acid or metaphosphoric acid.
9. The hydrocracking catalyst according to claim 8, characterized in that The aluminum source is pseudo-boehmite.
10. The hydrocracking catalyst according to claim 8, characterized in that The silicon source is water glass.
11. The hydrocracking catalyst according to claim 8, characterized in that The template agent is diethylamine.
12. The hydrocracking catalyst according to claim 1, characterized in that In step (3), the molar ratio of the aluminum source, phosphorus source, silicon source, template and water in the molecular sieve slurry is (1-3):(3-6):(0.5-2):(3-16):(100-360).
13. A method for preparing the hydrocracking catalyst according to any one of claims 1 to 12, characterized in that: include: The carrier is impregnated with an impregnation solution containing active metals, and then dried and calcined to obtain a hydrocracking catalyst; The impregnation process is to supersaturate the carrier with W-Ni complex impregnation liquid, and the active metals are calculated on the basis of the catalyst weight, with W oxide accounting for 10-30%, Ni oxide accounting for 3-8%, and P oxide accounting for 0.1-3%.