Titanium silicon molecular sieve and preparation method thereof and phenol hydroxylation method

By adding silanization reagents to titanium silica sol to prepare hierarchical porous titanium silica molecular sieves, the problem of insufficient mass transfer and diffusivity of titanium silica molecular sieves is solved, the conversion rate and selectivity of the phenol hydroxylation reaction are significantly improved, and the catalytic performance is improved.

CN116332194BActive Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202111579941.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-10-22
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Titanium silicon molecular sieve TS-1 has insufficient mass transfer and diffusivity when catalyzing the reaction of macromolecular hydrocarbons, which limits its catalytic performance. Especially in the phenol hydroxylation reaction, the catalytic oxidation performance needs to be improved.

Method used

By adding specific silanization reagents to titanium silica sol, hierarchical porous titanium silica molecular sieves are prepared through hydrothermal crystallization and roasting to improve its microporous structure and internal surface area, thus improving the activity and selectivity of phenol hydroxylation reaction.

Benefits of technology

The conversion rate and selectivity of the phenol hydroxylation reaction are significantly improved. The phenol conversion rate reaches more than 20%, and the selectivity of catechol and hydroquinone is increased to more than 40% respectively, improving the activity and selectivity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116332194B_ABST
    Figure CN116332194B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of phenol hydroxylation catalytic reaction, and specifically to titanium silicalite and its preparation method and phenol hydroxylation method, the method comprising: (1) uniformly mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalite; (2) adding a silanization agent to the titanium silicalite, and hydrothermally crystallizing and calcining the obtained mixture. The present invention treats the titanium silicalite precursor with a specific silanization agent, and the prepared titanium silicalite has high phenol hydroxylation activity when used in the catalytic phenol hydroxylation reaction, and the phenol conversion rate is significantly increased to more than 20%, the selectivity of catechol is increased to more than 40%, and the selectivity of hydroquinone is increased to more than 40%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of phenol hydroxylation catalytic reaction, and in particular to a titanium silicon molecular sieve and a preparation method thereof and a phenol hydroxylation method. Background Art

[0002] In the industrial production process, heterogeneous catalysts have attracted great attention from scientific researchers due to their advantages such as reusability and easy separation. Among them, molecular sieves, as typical representatives of heterogeneous catalysts, have also been widely developed and applied. Heteroatom molecular sieves refer to molecular sieves with regular topological structures in which specific metal atoms replace silicon atoms in all-silicon molecular sieves, enter the molecular sieve framework, and constitute catalytic active centers. In 1983, titanium silicon molecular sieve (TS-1) was first synthesized by Taramasso et al., which was regarded as a milestone in the field of molecular sieve catalysis. Subsequently, people prepared a variety of heteroatom (such as tin, iron, gallium, zirconium, vanadium, etc.) molecular sieve materials. In the environmentally friendly conversion reaction of oxygenated hydrocarbons, heteroatom molecular sieves show incomparable advantages over conventional methods. In particular, titanium silicon molecular sieves, in the selective oxidation reaction of hydrocarbons with hydrogen peroxide as the oxidant, show many advantages such as mild reaction conditions, high atom utilization, and environmentally friendly and pollution-free process. It has great prospects for industrial application and has always been the focus of researchers.

[0003] At present, Ti heteroatom molecular sieves represented by TS-1 molecular sieve have been successfully applied to industrial production processes such as propylene liquid phase epoxidation and cyclohexanone ammoxidation. However, the titanium silicalite molecular sieve TS-1 has a ten-membered ring channel with an MFI structure and a pore size of about 0.55nm, which may limit the diffusion and mass transfer of macromolecular hydrocarbons and restrict its application. Therefore, improving the mass transfer and diffusion properties of TS-1 molecular sieve is conducive to improving its performance in catalyzing macromolecular reactants. In recent years, the synthesis of multi-level porous titanium silicalite molecular sieves with both micropores and mesopores has become a research focus. It not only has sufficient framework Ti atoms, but also the mesopores can effectively promote the intracrystalline diffusion and mass transfer effect of the reaction molecules. So far, there are many methods for preparing multi-level porous titanium silicalite molecular sieves, such as alkali dissolution method, hard / soft template method, silanization agent layer method, etc. Among them, the silanization agent layer method is an effective method for preparing multi-level porous titanium silicalite molecular sieves.

[0004] CN108726528A discloses a multi-level porous titanium silicalite molecular sieve and a preparation method thereof and a method for olefin epoxidation. A certain proportion of mesoporous channels can be introduced into the titanium silicalite molecular sieve by treatment with a silanization agent, but the catalytic oxidation performance of the molecular sieve needs to be further improved. Summary of the invention

[0005] The purpose of the present invention is to improve the catalytic oxidation performance of titanium silicalite in the phenol hydroxylation reaction, and to provide titanium silicalite and a preparation method thereof and a phenol hydroxylation method.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing titanium silicon molecular sieve, the method comprising:

[0007] (1) mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalose;

[0008] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0009]

[0010] Wherein, i is an integer of 1-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0011] The second aspect of the present invention provides a titanium silicon molecular sieve prepared according to the method described in the first aspect.

[0012] The third aspect of the present invention provides a method for hydroxylating phenol, the method comprising: contacting phenol with a catalyst and hydrogen peroxide for reaction, wherein the catalyst comprises the titanium silicalite described in the second aspect.

[0013] Through the above technical scheme, the present invention treats the titanium silicalite precursor with a specific silanization reagent, and the prepared titanium silicalite has high phenol hydroxylation activity when used in the catalytic phenol hydroxylation reaction, and the phenol conversion rate is significantly improved to more than 20%, the selectivity of catechol is improved to more than 40%, and the selectivity of hydroquinone is improved to more than 40%. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is the XRD spectrum of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0015] Figure 2 is the UV-Vis spectrum of the titanium silicate molecular sieve obtained in Example 1 of the present invention;

[0016] Figure 3 is a TEM image of the titanium silicon molecular sieve obtained in Example 1 of the present invention;

[0017] Figure 4 This is the XRD spectrum of the titanium silicon molecular sieve obtained in Comparative Example 1. DETAILED DESCRIPTION

[0018] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0019] As mentioned above, the first aspect of the present invention provides a method for preparing titanium silicon molecular sieve, the method comprising:

[0020] (1) mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalose;

[0021] (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination;

[0022]

[0023] Wherein, i is an integer of 1-10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group.

[0024] In the present invention, the C1-C6 alkyl group refers to an alkyl group having 1 to 6 carbon atoms in total, for example, it can be one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl and n-hexyl.

[0025] In some preferred embodiments of the present invention, i is an integer of 1-5, for example, 1, 2, 3, 4 or 5.

[0026] In some preferred embodiments of the present invention, R1, R2 and R3 are each independently selected from a C1-C3 alkyl group, and the C1-C3 alkyl group may be a methyl group, an ethyl group, a n-propyl group or an isopropyl group. Preferably, R1, R2 and R3 are each independently selected from a methyl group, an ethyl group or an n-propyl group. In the present invention, R1, R2 and R3 may be the same or different. Preferably, R1, R2 and R3 are the same.

[0027] In the present invention, by adding a specific silanization agent (the compound shown in formula (I)) to the titanium silicalite sol, the electrostatic force between the thiol groups in multiple silanization agents is used to make the titanium silicalite molecular sieve obtained by crystallization have a richer microporous structure; during the phenol hydroxylation reaction, it is beneficial to the intra-crystal and inter-crystal mass transfer and diffusion of the reactant molecules and the product molecules, thereby effectively improving the reaction effect.

[0028] According to the present invention, if the amount of the silanization agent (the compound shown in formula (I)) is too high, the crystallization performance of the titanium silical sol will be deteriorated and the molecular sieve skeleton structure will be imperfect; and if the amount of the silanization agent (the compound shown in formula (I)) is too low, the internal surface area of ​​the obtained titanium silicalite molecular sieve will be reduced, affecting mass transfer and further affecting its activity in catalyzing the hydroxylation reaction of phenol; according to the present invention, under preferred conditions, in step (1), the silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound shown in formula (I) is 1:(0.01-0.3), preferably 1:(0.01-0.2); more preferably 1:(0.05-0.1).

[0029] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and the alkaline template is calculated as OH when it does not contain nitrogen. - The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); preferably 1:(0.1-0.3):(5-25).

[0030] According to the present invention, under preferred conditions, the silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, white carbon black and silica sol.

[0031] According to the present invention, under preferred conditions, the alkaline template is selected from at least one of quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines, preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

[0032] In some preferred embodiments of the present invention, the silicon source is calculated as SiO2, the titanium source is calculated as TiO2, and the molar ratio of the silicon source to the titanium source is 1:(0.001-0.04), preferably 1:(0.005-0.025).

[0033] According to the present invention, under preferred conditions, the titanium source is selected from an organic titanium source and / or an inorganic titanium source; further preferably, the titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

[0034] In a preferred embodiment of the present invention, step (1) further comprises: mixing the silicon source, the alkaline template and water, and performing a first stirring at room temperature for 0.1-2 hours, then adding the titanium source during the stirring process, and performing a second stirring for 0.5-6 hours to obtain titanium silicalose. Under preferred conditions, the second stirring time is 0.5-3 hours, more preferably 1-3 hours.

[0035] According to the present invention, under preferred conditions, step (1) further comprises: driving out alcohol after the mixing; driving out alcohol can remove alcohol generated by hydrolysis of silicon source and titanium source, and in the present invention, preferably azeotropic distillation is used to remove alcohol generated in the system, and water lost by azeotropic distillation is supplemented during the driving out alcohol process to ensure that the ratio of each substance in the titanium silica sol meets the above requirements; preferably, the conditions for driving out alcohol include: temperature of 30-100°C and time of 2-10h; more preferably: temperature of 40-90°C and time of 4-10h.

[0036] According to the present invention, in order to make the silanization agent (the compound represented by formula (I)) be uniformly dispersed in the titanium silica sol, under preferred conditions, step (1) also includes: adding the compound represented by formula (I) to the titanium silica sol and performing a third stirring for 0.1-24 hours, preferably the third stirring time is 0.5-10 hours, and more preferably 3-5 hours.

[0037] In the present invention, the nucleation and growth process of the molecular sieve can be controlled by rapidly heating, thereby obtaining molecular sieve particles of smaller size; according to the present invention, under preferred conditions, in step (2), the conditions for hydrothermal crystallization include: heating the mixture to 50-200°C within 0.1-1h, and then performing hydrothermal crystallization at 50-200°C for 10-100h; preferably, performing hydrothermal crystallization at a temperature of 100-200°C for 10-80h; further preferably, the heating time is 0.1-0.5h; more preferably, the conditions for hydrothermal crystallization include: a temperature of 120-200°C and a time of 20-70h; under the above preferred conditions, the specific surface area and pore volume of the molecular sieve can be balanced; and a molecular sieve with a specific specific surface area and pore volume is prepared.

[0038] The present invention has no particular limitation on the pressure of hydrothermal crystallization, which may be the autogenous pressure of the crystallization system.

[0039] According to the present invention, under preferred conditions, the method further comprises: washing, filtering and drying the product obtained by hydrothermal crystallization; wherein the washing, filtering and drying processes can be known to those skilled in the art. Exemplarily, the washing temperature can be 20-50°C, the washing solvent can be water, and the amount of the washing solvent is 1-20 times the mass of the crystallized product; the drying conditions can be: the temperature is 40-150°C and the time is 0.5-24h.

[0040] In some preferred embodiments of the present invention, the calcination conditions include: a temperature of 400-800° C. and a time of 1-15 h; preferably a temperature of 500-600° C. and a time of 4-10 h.

[0041] The second aspect of the present invention provides a titanium silicon molecular sieve prepared according to the method described in the first aspect.

[0042] Preferably, the UV-Vis characteristic peak of the titanium silicate molecular sieve is located at 210-230 nm; the micropore volume is 0.34-0.37 cm 3 / g; internal surface area is 430-480m 2 / g.

[0043] In the present invention, the internal surface area refers to the specific surface area of ​​the internal pore structure contained in the molecular sieve.

[0044] The third aspect of the present invention provides a method for hydroxylating phenol, the method comprising: contacting phenol with a catalyst and hydrogen peroxide for reaction, wherein the catalyst comprises the titanium silicalite described in the second aspect.

[0045] According to the present invention, under preferred conditions, the conditions for phenol hydroxylation include: temperature of 30-120°C, molar ratio of phenol to hydrogen peroxide of (2-5):1, and weight ratio of titanium silicalite to phenol of (0.01-0.1):1.

[0046] The form of the catalyst can be selected according to actual needs. The catalyst can be a molecular sieve supported on a carrier or a molecular sieve powder. In the present invention, it is preferred to directly use the molecular sieve powder as the catalyst.

[0047] According to a particularly preferred embodiment of the present invention, the method for preparing titanium silicon molecular sieve comprises:

[0048] (1) mixing a silicon source, an alkaline template and water in a molar ratio of 1:(0.1-0.3):(5-25), performing a first stirring at room temperature for 0.1-2 hours, then adding a titanium source during the stirring process, and then performing a second stirring for 0.5-6 hours to obtain a mixed system; wherein the molar ratio of the silicon source to the titanium source is 1:(0.005-0.025);

[0049] Then, the mixed system is subjected to alcohol removal to obtain titanium silicalose; the temperature of the alcohol removal is 40-90° C. and the time is 4-10 hours;

[0050] (2) adding the compound represented by formula (I) to the titanium silicalose, and subjecting the obtained mixture to hydrothermal crystallization and calcination; wherein the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.3), and the crystallization conditions are: heating the mixture to 120-200° C. within 0.1-0.5 h, and then subjecting the mixture to hydrothermal crystallization at 120-200° C. for 20-70 h;

[0051]

[0052] Wherein, i is an integer of 1-5; R1, R2 and R3 are the same; R1, R2 and R3 are selected from ethyl or propyl.

[0053] The present invention will be described in detail below by way of examples. In the following examples, room temperature refers to 25±5°C.

[0054] In the following examples and comparative examples, the X-ray diffraction (XRD) crystal phase diagram of the samples was measured on a Siemens D5005 X-ray diffractometer, with a ray source of Cu Kα, a tube voltage of 40 kV, a tube current of 40 mA, a scanning speed of 0.5° / min, and a scanning range of 2θ=5°-35°;

[0055] The UV-Vis spectra (UV-Vis) of the samples were obtained by Agilent Cary 300 UV spectrophotometer with a wavelength interval of 3 nm and a scanning range of 190-800 nm;

[0056] Transmission electron microscopy (TEM) characterization images were measured using JEOL JEM-2100;

[0057] The internal surface area was obtained by measuring the static N2 adsorption-desorption curve of the sample at liquid nitrogen temperature (77.4 K) using Micromeritics' ASAP2405J static nitrogen adsorption instrument, and then performing BET fitting on the adsorption curve in the range of P / P0 = 0.05 to 0.35;

[0058] The pore volume was determined according to the method described in RIPP 151-90 in "Analytical Methods in Petrochemical Industry" compiled by Yang Cuiding et al. (Science Press, first edition, published in September 1990).

[0059] In the following examples, the chemical structural formulas of the silanization agents used are shown in Table 1, wherein Compound 1, Compound 2 and Compound 3 were all commercially available.

[0060] Table 1

[0061]

[0062] Example 1

[0063] (1) Tetraethyl silicate, tetrapropylammonium hydroxide and water are stirred and mixed at room temperature, and tetrabutyl titanate is added during the stirring process, and a second stirring is performed for 2 hours to obtain a mixed system; wherein tetraethyl silicate is calculated as SiO2, tetrapropylammonium hydroxide is calculated as N, and tetrabutyl titanate is calculated as TiO2, and the molar ratio of tetraethyl silicate, tetrapropylammonium hydroxide, water and tetrabutyl titanate is 1:0.2:20:0.015;

[0064] Then, the mixed system was subjected to alcoholization at 70°C for 6 hours to obtain titanium silicalose;

[0065] (2) adding compound (1) to the titanium silicalose, and stirring for a third time at room temperature for 5 hours to obtain a mixture, wherein the molar ratio of compound 1 to tetraethyl silicate is 0.1:1;

[0066] (3) heating the mixture to 160° C. for 0.5 h, and performing hydrothermal crystallization at 160° C. for 72 h to obtain a crystallized product;

[0067] The crystallized product was sequentially washed with water, filtered, and dried at 120 °C for 2 h;

[0068] The dried product was calcined at 550°C for 6 hours to obtain titanium silicon molecular sieve;

[0069] The XRD spectrum of the titanium silicon molecular sieve obtained in this example is as follows: Figure 1 As shown, the UV-Vis spectrum is Figure 2 As shown in the TEM image Figure 3 The physical parameters are shown in Table 3. Figure 1 It can be seen that the titanium silicon molecular sieve prepared in this example has an MFI structure and good crystallinity; Figure 2 The peak at 220 nm is a characteristic peak of a tetracoordinated titanium atom, indicating that the titanium silicon molecular sieve prepared in this example has a framework titanium active center. Figure 3 It can be seen that the particle size of the titanium silicon molecular sieve prepared in this example is about 250 nm.

[0070] Embodiment 2-20

[0071] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportions and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0072] Comparative Example 1

[0073] Titanium silicate molecular sieve was prepared according to the method for preparing titanium silicate micro-mesoporous molecular sieve composite material disclosed in "Zeolites, 1992, Vol. 12, pp. 943-950". The specific method is as follows:

[0074] Mix 22.5g of tetraethyl silicate, 7g of tetrapropylammonium hydroxide and 59.8g of deionized water evenly and hydrolyze at 60°C for 1h. Then, slowly drip a solution consisting of 1.1g of tetrabutyl titanate and 5g of isopropanol into the above solution under vigorous stirring, and stir the mixture at 75°C for 3h to obtain a clear and transparent colloid. Then move the colloid into a stainless steel closed reactor and crystallize it at a constant temperature of 170°C for 72h to obtain a conventional TS-1 molecular sieve. Its XRD analysis spectrum is shown as follows: Figure 4shown.

[0075] Comparative Examples 2-6

[0076] Titanium silicate molecular sieve was prepared according to the method of Example 1. The proportion and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0077] Comparative Example 7

[0078] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent was methyltriethoxysilane (Compound 4), the raw material ratio and synthesis conditions were shown in Table 2, and the physical properties of the prepared molecular sieve were shown in Table 3.

[0079] Comparative Example 8

[0080] Titanium silicate molecular sieve was prepared according to the method of Example 1, except that the silanization agent was N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (Compound 5). The raw material ratio and synthesis conditions are shown in Table 2. The physical properties of the prepared molecular sieve are shown in Table 3.

[0081]

[0082] Table 3

[0083]

[0084] Test Case

[0085] This test example illustrates the reaction effect of the sample of the embodiment provided by the present invention and the sample prepared in the comparative example for the hydroxylation of phenol to prepare diphenol. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is a FFAP column.

[0086] In the test example, the phenol conversion rate and the hydroquinone selectivity were calculated according to the following formulas:

[0087] Phenol conversion rate % = (1-the number of moles of phenol remaining after the reaction / the number of moles of phenol added before the reaction) * 100%

[0088] Hydroquinone selectivity % = moles of hydroquinone after reaction / (moles of phenol added before reaction - moles of phenol remaining after reaction) * 100%

[0089] 1.25 g of each sample prepared in the above Examples 1-20 and Comparative Examples 1-8 was added to a three-necked flask reaction vessel containing 25 g of phenol and 20 ml of acetone. After the temperature was stabilized to the set value, 9.81 g of hydrogen peroxide was added, and the molar ratio of phenol: hydrogen peroxide (in terms of H2O2) was 3:1. Then, the phenol hydroxylation reaction was carried out at a temperature of 80°C and a pressure of 0.1 MPa (normal pressure) for 2 hours. Then, sampling was performed, and the phenol conversion rate, catechol selectivity and hydroquinone selectivity were analyzed. The results are shown in Table 4.

[0090] Table 4

[0091]

[0092]

[0093] As can be seen from Table 4, the sample obtained by the present invention can be used as a catalyst for the hydroxylation reaction of phenol, which can significantly increase the conversion rate of phenol to 27%, the selectivity of catechol to 48%, and the selectivity of hydroquinone to 48%, and has a better catalytic effect.

[0094] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing titanium silicon molecular sieve, characterized in that: The method comprises: (1) mixing a silicon source, an alkaline template, a titanium source and water to obtain a titanium silicalose; (2) adding the compound represented by formula (I) to the titanium silicalose sol, and subjecting the obtained mixture to hydrothermal crystallization and calcination; wherein i is an integer from 1 to 10; R1, R2 and R3 are each independently selected from a C1-C6 alkyl group; The UV-vis characteristic peak of the titanium silicate molecular sieve prepared by the method is located at 210-230nm; the micropore volume is 0.34-0.37cm 3 / g; internal surface area is 430-480m 2 / g.

2. The method according to claim 1, wherein: i is an integer from 1 to 5.

3. The method according to claim 1, wherein: R1, R2 and R3 are each independently selected from methyl, ethyl or propyl.

4. The method according to claim 1, wherein: The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.3).

5. The method according to claim 4, wherein: The silicon source is calculated as SiO2, and the molar ratio of the silicon source to the compound represented by formula (I) is 1:(0.01-0.2).

6. The method according to any one of claims 1 to 5, wherein: The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.05-0.4):(5-40); The molar ratio of the silicon source to the titanium source is 1:(0.001-0.04).

7. The method according to claim 6, wherein: The silicon source is calculated as SiO2, the alkaline template is calculated as N when it contains nitrogen, and as OH when it does not contain nitrogen. - The titanium source is calculated as TiO2, The molar ratio of the silicon source, the alkaline template and water is 1:(0.1-0.3):(5-25); The molar ratio of the silicon source to the titanium source is 1:(0.005-0.025).

8. The method according to any one of claims 1 to 5, wherein: The silicon source is selected from at least one of tetramethyl silicate, tetraethyl silicate, tetrapropyl silicate, tetrabutyl silicate, white carbon black and silica sol.

9. The method according to any one of claims 1 to 5, wherein: The alkaline template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

10. The method according to claim 9, wherein: The alkaline template agent is selected from at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

11. The method according to any one of claims 1 to 5, wherein: The titanium source is selected from an organic titanium source and / or an inorganic titanium source.

12. The method according to claim 11, wherein: The titanium source is selected from at least one of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate.

13. The method according to any one of claims 1 to 5, wherein: Step (1) also includes removing alcohol after the mixing; The conditions for driving out the alcohol include: temperature of 30-100° C. and time of 2-10 h.

14. The method according to claim 13, wherein: The conditions for driving out the alcohol include: temperature of 40-90° C. and time of 4-10 h.

15. The method according to any one of claims 1 to 5, wherein: In step (2), the hydrothermal crystallization conditions include: heating the mixture to 50-200° C. within 0.1-1 h, and then crystallizing at 50-200° C. for 10-100 h.

16. The method according to claim 15, wherein: In step (2), the hydrothermal crystallization conditions include: performing crystallization at a temperature of 100-200° C. for 20-80 hours.

17. The method according to any one of claims 1 to 5, wherein: The calcination conditions include: temperature of 400-800° C. and time of 1-15 hours.

18. A titanium silicon molecular sieve prepared according to the method according to any one of claims 1 to 17.

19. A method for hydroxylating phenol, the method comprising: Phenol is contacted with a catalyst and hydrogen peroxide for reaction, wherein the catalyst comprises the titanium silicon molecular sieve according to claim 18.

20. The method according to claim 19, wherein: The conditions for phenol hydroxylation include: a temperature of 30-120° C., a molar ratio of phenol to hydrogen peroxide of (2-5):1, and a weight ratio of titanium silicalite to phenol of (0.01-0.1):1.

Citation Information

Patent Citations

  • Hierarchical porous titanium-silicon molecular sieve as well as preparation method thereof and olefin epoxidation method

    CN108726528A

  • Titanium silicon zeolite loaded with small-size gold nanoparticles and preparation method of titanium silicon zeolite

    CN109399659A

  • Packaged platinum group sub-nanometallic supported porous-grade titanium silicon molecular sieve catalyst as well as preparation and application thereof

    CN109999902A

  • Preparation method of mesoporous microporous composite titanium-silicon material loaded Au-Pd nano-catalyst

    CN111957311A

  • Preparation method and application of sulfydryl functionalized MCM molecular sieve

    CN112320815A