A kind of anti-aging type silicone tube for ventilation and water circulation and preparation method thereof

By using a composite anti-aging agent in silicone tubing, combining inorganic and organic anti-aging mechanisms, the problem of insufficient aging resistance of silicone tubing is solved, flame retardant performance is improved, and application scenarios are broadened.

CN116333495BActive Publication Date: 2024-11-19HEFEI HENGDECHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310487319.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-19
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

Existing silicone tubing has insufficient aging resistance and unsatisfactory flame retardancy, which limits its application in ventilation and water supply pipes.

Method used

A composite anti-aging agent is used, which grafts organic anti-aging additives onto the surface of inorganic ultraviolet light shielding agents nano-ZnO and nano-TiO2 to form an organic coating layer. This combines inorganic and organic anti-aging mechanisms to improve dispersibility and flame retardant properties.

Benefits of technology

This improves the aging resistance and flame retardant properties of silicone tubing, broadens its application scenarios, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004208954600000031
    Figure BDA0004208954600000031
  • Figure BDA0004208954600000032
    Figure BDA0004208954600000032
  • Figure BDA0004208954600000041
    Figure BDA0004208954600000041
Patent Text Reader

Abstract

The invention discloses an anti-aging type silicone tube for ventilation and water circulation and a preparation method thereof, belongs to the technical field of silicone tubes, and includes the following raw materials by weight: 100 parts of silicone rubber, 30-40 parts of white carbon black, 2-3 parts of vulcanizing agent, 6-9 parts of phenyl silicone oil, 11-15 parts of composite anti-aging agent, and 4-7 parts of methyl silicone resin. The present invention adds a composite anti-aging agent to the raw material of the silicone tube, can combine inorganic and organic anti-aging action mechanisms, and comprehensively combine the advantages of the two, and has stable and efficient anti-aging performance; through grafting and compounding, a layer of organic wrapping layer can be formed on the surface of the inorganic anti-aging filler, promoting the uniform dispersion of the composite anti-aging agent in the silicone rubber; the composite anti-aging agent has a certain flame retardant effect, can improve the flame retardant performance of the silicone tube to a certain extent, so that the obtained silicone tube can be used for water ventilation, improve service life, and can broaden the application scene of the silicone tube.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of silicone tubes, and in particular, relates to an anti-aging silicone tube for ventilation and water circulation and a preparation method thereof. Background Art

[0002] Silicone tubes are carriers for the circulation and coating of liquids, gases and other materials. In the industry, silicone rubber tubes can be divided into extruded tubes and special-shaped tube strips, which are widely used in modern industry, national defense industry and daily necessities. Silicone tubes are made by adding raw silicone rubber to a double-roll rubber mixer or a closed kneading machine, gradually adding white carbon black and other additives, and repeatedly refining them evenly, and then extruding them into products. At present, silicone tubes have the technical problem of insufficient aging resistance.

[0003] In the prior art, light stabilizers or UV shielding agents are often added to silicone rubber to improve the aging resistance of silicone rubber. Light stabilizers are generally organic UV absorbers, which have the disadvantage of being not stable enough. UV shielding agents are generally inorganic fillers that can shield UV light, which have the disadvantage of being easy to agglomerate and having poor compatibility with the matrix interface, making it difficult to disperse evenly, affecting the anti-aging effect and the mechanical properties of the silicone finished product. Therefore, the anti-aging treatment method for silicone needs to be further improved. In addition, as a polymer material, silicone rubber is not very flame retardant, which limits its use scenarios when used in ventilation and water pipes. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide an aging-resistant silicone tube for ventilation and water circulation and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An aging-resistant silicone tube for ventilation and water circulation, comprising the following raw materials in parts by weight: 100 parts of silicone rubber, 30-40 parts of white carbon black, 2-3 parts of vulcanizing agent, 6-9 parts of phenyl silicone oil, 11-15 parts of composite antioxidant, and 4-7 parts of methyl silicone resin;

[0007] The preparation method of the aging-resistant silicone tube comprises the following steps:

[0008] The first step is to add silicone rubber, white carbon black, phenyl silicone oil and methyl silicone resin into a vacuum kneader, mix them evenly at room temperature, and then evacuate at 180°C for 2-3 hours to make a silicone rubber compound;

[0009] Step 2: Add the composite antioxidant to the silicone rubber compound, then mix it evenly in a vacuum kneader, then add the vulcanizing agent, and mix it evenly on an open mill;

[0010] The third step is to cut the mixed rubber into small strips and extrude them on an extruder, and then vulcanize and shape them in a hot air drying tunnel or in a molding device to make a silicone tube.

[0011] Furthermore, the vulcanizing agent is any one of 2,4-dichlorobenzoyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane), and diisopropylbenzene peroxide.

[0012] Furthermore, the composite antioxidant is prepared by the following steps:

[0013] S1. In a three-necked flask equipped with a thermometer, an electric stirrer, a water separator and a reflux condenser, 5-nitroisophthalic acid and pentamethylpiperidinol were added, and then p-toluenesulfonic acid (catalyst) and toluene (water agent) were added, and the mixture was heated under constant stirring, heated to reflux at 126-130° C. for 2.5 h, and then kept warm for 1 h. The reaction solution was cooled, and toluene was removed by distillation under reduced pressure. The organic phase was then washed with saturated brine and saturated sodium carbonate solution for several times, and the crude product was recrystallized from ethanol to obtain intermediate 1; the amount ratio of 5-nitroisophthalic acid, pentamethylpiperidinol, p-toluenesulfonic acid and toluene was 10.6 g:17.1 g:1.4 g:40 mL;

[0014] Add intermediate 1 and toluene to a reactor, add palladium carbon catalyst, evacuate the air in the reactor under reduced pressure, then introduce hydrogen, and carry out reduction reaction at a pressure of 2 atm for 3 hours. After the reaction is completed, filter, and remove toluene from the filtrate under reduced pressure to obtain intermediate 2; the amount of palladium carbon catalyst added is 20 μg / g of the mass of intermediate 1;

[0015] 5-Nitroisophthalic acid and pentamethylpiperidinol undergo esterification reaction to obtain intermediate 1. The -NO2 on the intermediate 1 molecule is then reduced by hydrogen to form -NH2 to obtain intermediate 2. The process is as follows:

[0016]

[0017] S2, add intermediate 2, triethylamine and benzene to a dry three-necked flask, place the flask in an ice bath, stir and mix, when the system temperature is stabilized at 0-2 ° C, slowly dropwise add a benzene solution of cyanuric chloride under stirring, react for 3 hours at 0-2 ° C after the addition is complete, filter to remove the generated salt, remove the solvent by vacuum rotary evaporation, and purify by column chromatography (using a mixed solvent of n-hexane-ethyl acetate as an eluent, the volume ratio of the two is 11:9), and spin-dry the eluent to obtain intermediate 3; the ratio of the amount of intermediate 2, triethylamine and cyanuric chloride is 43.9g:9.1g:5.5g;

[0018] The -NH2 on the intermediate 2 molecule undergoes a nucleophilic substitution reaction with the -Cl on the cyanuric chloride molecule. By controlling the molar ratio of the two to 3:1, a tri-substitution reaction occurs. The process is shown below to obtain intermediate 3:

[0019]

[0020] S3, remove the air in the four-necked flask with N2, add 4-chlorobutyric acid and acetone, stir and mix evenly, place in an ice-water bath, slowly drop triethylamine and benzene solution of intermediate 3 while stirring, after the dropwise addition is complete, heat to 40 ° C and react for 4h, remove triethylamine hydrochloride by suction filtration, and obtain an anti-aging additive after the filtrate is distilled under reduced pressure; the ratio of 4-chlorobutyric acid, intermediate 3 and triethylamine is 6.2g:28.1g:5.1g;

[0021] The -NH- on the intermediate 3 undergoes a nucleophilic substitution reaction with the -Cl on the 4-chlorobutyric acid molecule to obtain an anti-aging additive. The reaction process is as follows:

[0022]

[0023] S4. Add γ-aminopropyltriethoxysilane and ethanol aqueous solution (volume fraction is 60%) into a round-bottom flask, mix and dissolve evenly, then add anti-aging filler, ultrasonicate for 10 minutes, reflux and stir at 82°C for 2 hours, centrifuge, wash the product with ethanol aqueous solution 3-4 times, and finally vacuum dry at 60°C, grind, and obtain pretreated filler; the ratio of anti-aging filler, γ-aminopropyltriethoxysilane, and ethanol aqueous solution is 1g:15mL:100mL;

[0024] The surface of the anti-aging filler is treated by hydrolyzing γ-aminopropyltriethoxysilane, and a molecular chain containing amino groups is grafted on the surface to obtain a pretreated filler;

[0025] The anti-aging filler is a compound of nano ZnO and nano TiO2 in a mass ratio of 2:1-2; both nano ZnO and nano TiO2 are ultraviolet light shielding agents, which can not only effectively absorb and scatter UVA and UVB ultraviolet rays, but also have light stability and chemical stability.

[0026] S5. Add the pretreated filler and DMF (N,N-dimethylformamide) into a three-necked flask with a stirring device. After mechanically stirring at room temperature for 1 hour, add the anti-aging agent into the system and continue stirring for 30 minutes. Then add EDC-HCl (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, coupling agent). Transfer the mixed solution to a 60°C water bath and continue stirring and reacting for 4 hours. After the reaction is completed, centrifuge and wash with ethanol aqueous solution for 4-5 times. Finally, fully dry the product in a 60°C vacuum oven and grind it to obtain a composite anti-aging agent. The ratio of the pretreated filler, anti-aging agent and EDC-HCl is 10g:26.5g:0.1g.

[0027] The -COOH contained in the anti-aging agent molecule undergoes an amidation reaction with the -NH2 introduced on the surface of the pretreated filler, and the anti-aging agent molecule chain is grafted onto the surface of the anti-aging filler to obtain a composite anti-aging agent.

[0028] The obtained composite antioxidant uses anti-aging fillers (nano ZnO and nano TiO2) as a matrix, and anti-aging additives are grafted on the surface of the matrix through chemical bonding. Firstly, the matrix of the composite antioxidant is an inorganic ultraviolet shielding agent, which can not only effectively absorb and scatter UVA and UVB ultraviolet rays, but also has light stability and chemical stability. The surface-grafted anti-aging additive is an organic hindered amine light stabilizer, which can effectively capture free radicals in the polymer degradation chain reaction to achieve anti-aging effects. Therefore, the composite antioxidant can combine the inorganic and organic anti-aging action mechanisms, combine the advantages of the two, and have stable and efficient anti-aging performance. In addition, through grafting and compounding, an organic coating layer can be formed on the surface of the inorganic anti-aging filler, which can It can effectively improve the uniform dispersion of inorganic anti-aging fillers in silicone rubber, and contains multiple benzene rings and cyanuric rings with high steric hindrance effect. The steric hindrance effect can improve the agglomeration phenomenon between inorganic anti-aging fillers and further promote dispersion. It should be noted that the anti-aging agent molecule contains multiple hindered amine groups. The higher the density of the hindered amine, the better the anti-aging effect. Therefore, the anti-aging performance of the composite antioxidant is further improved. In addition, due to the presence of cyanuric rings and benzene rings in the anti-aging agent, the cyanuric ring decomposes through endothermic decomposition and generates non-flammable gases (NO, NO2, etc.) to dilute combustibles and play a flame retardant role. The benzene ring promotes carbonization. Therefore, the anti-aging agent has a certain flame retardant effect and can improve the flame retardant properties of silicone tubes to a certain extent.

[0029] Beneficial effects of the present invention:

[0030] The present invention adds a composite antioxidant to the raw materials of the silicone tube, which can combine the inorganic and organic anti-aging action mechanisms, integrate the advantages of the two, and have stable and efficient anti-aging performance; through grafting and compounding, an organic coating layer can be formed on the surface of the inorganic anti-aging filler, promoting the uniform dispersion of the composite antioxidant in the silicone rubber; the composite antioxidant has a certain flame retardant effect, can improve the flame retardant performance of the silicone tube to a certain extent, so that the obtained silicone tube can be used for water and ventilation, improve the service life, and can broaden the application scenarios of the silicone tube. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] Preparation of composite antioxidant:

[0034] S1. In a three-necked flask equipped with a thermometer, an electric stirrer, a water separator and a reflux condenser, 10.6 g of 5-nitroisophthalic acid and 17.1 g of pentamethylpiperidinol were added, and then 1.4 g of p-toluenesulfonic acid (catalyst) and 40 mL of toluene (with water) were added. The mixture was heated under constant stirring at 126 ° C. and refluxed for 2.5 h, and then kept warm for 1 h. The reaction solution was cooled, and toluene was removed by distillation under reduced pressure. The organic phase was then washed with saturated brine and saturated sodium carbonate solution for multiple times. The crude product was recrystallized from ethanol to obtain intermediate 1.

[0035] 25.9 g of intermediate 1 and toluene were added to a reactor, and 518 μg of palladium-carbon catalyst was added. The air in the reactor was evacuated under reduced pressure, and then hydrogen was introduced under a pressure of 2 atm to carry out a reduction reaction for 3 h. After the reaction was completed, the reaction was filtered, and the filtrate was evaporated under reduced pressure to remove toluene to obtain intermediate 2;

[0036] S2, add 43.9g of intermediate 2, 9.1g of triethylamine and 120mL of benzene to a dry three-necked flask, place the flask in an ice bath, stir and mix, when the system temperature is stable at 0°C, slowly drop 25mL of a benzene solution containing 5.5g of cyanuric chloride under stirring, react at 0°C for 3h after the addition is complete, filter to remove the generated salt, remove the solvent by vacuum rotary evaporation, and purify by column chromatography (using a mixed solvent of n-hexane-ethyl acetate as the eluent, the volume ratio of the two is 11:9), spin-dry the eluent to obtain intermediate 3;

[0037] S3, remove the air in the four-necked flask with N2, add 6.2g of 4-chlorobutyric acid and 50mL of acetone, stir and mix evenly, place in an ice-water bath, and slowly drop 5.1g of triethylamine and 45mL of benzene solution containing 28.1g of intermediate 3 while stirring. After the addition is complete, heat to 40°C and react for 4h, remove triethylamine hydrochloride by suction filtration, and obtain an anti-aging additive after the filtrate is distilled under reduced pressure;

[0038] S4, add 45mL of γ-aminopropyltriethoxysilane and 300mL of ethanol aqueous solution (volume fraction of 60%) into a round-bottom flask, mix and dissolve evenly, then add anti-aging filler (a compound of 2g of nano ZnO and 1g of nano TiO2), ultrasonicate for 10min, reflux and stir at 82°C for 2h, centrifuge, wash the product with ethanol aqueous solution 3 times, and finally vacuum dry at 60°C, grind to obtain pretreated filler;

[0039] S5. Add 10g of pretreated filler and DMF into a three-necked flask with a stirring device. After mechanical stirring at room temperature for 1h, add 26.5g of anti-aging agent into the system and continue stirring for 30min. Then add 0.1g of EDC-HCl, transfer the mixture to a 60℃ water bath and continue stirring and reacting for 4h. After the reaction is completed, centrifuge and wash with ethanol aqueous solution 4 times. Finally, dry the product in a vacuum oven at 60℃ and grind it to obtain a composite anti-aging agent.

[0040] Example 2

[0041] Preparation of composite antioxidant:

[0042] S1. In a three-necked flask equipped with a thermometer, an electric stirrer, a water separator and a reflux condenser, 10.6 g of 5-nitroisophthalic acid and 17.1 g of pentamethylpiperidinol were added, and then 1.4 g of p-toluenesulfonic acid (catalyst) and 40 mL of toluene (with water) were added. The mixture was heated under constant stirring and refluxed at 130 ° C for 2.5 h, and then kept warm for 1 h. The reaction solution was cooled, and toluene was removed by distillation under reduced pressure. The organic phase was then washed with saturated brine and saturated sodium carbonate solution for multiple times. The crude product was recrystallized from ethanol to obtain intermediate 1.

[0043] 25.9 g of intermediate 1 and toluene were added to a reactor, and 518 μg of palladium-carbon catalyst was added. The air in the reactor was evacuated under reduced pressure, and then hydrogen was introduced under a pressure of 2 atm to carry out a reduction reaction for 3 h. After the reaction was completed, the reaction was filtered, and the filtrate was evaporated under reduced pressure to remove toluene to obtain intermediate 2;

[0044] S2, add 43.9g of intermediate 2, 9.1g of triethylamine and 120mL of benzene to a dry three-necked flask, place the flask in an ice bath, stir and mix, when the system temperature is stable at 2°C, slowly drop 25mL of a benzene solution containing 5.5g of cyanuric chloride under stirring, react at 2°C for 3h after the addition is complete, filter to remove the generated salt, remove the solvent by vacuum rotary evaporation, and purify by column chromatography (using a mixed solvent of n-hexane-ethyl acetate as the eluent, the volume ratio of the two is 11:9), spin-dry the eluent to obtain intermediate 3;

[0045] S3, remove the air in the four-necked flask with N2, add 6.2g of 4-chlorobutyric acid and 50mL of acetone, stir and mix evenly, place in an ice-water bath, and slowly drop 5.1g of triethylamine and 45mL of benzene solution containing 28.1g of intermediate 3 while stirring. After the addition is complete, heat to 40°C and react for 4h, remove triethylamine hydrochloride by suction filtration, and obtain an anti-aging additive after the filtrate is distilled under reduced pressure;

[0046] S4, add 60mL of γ-aminopropyltriethoxysilane and 400mL of ethanol aqueous solution (volume fraction of 60%) into a round-bottom flask, mix and dissolve evenly, then add anti-aging filler (a compound of 2g of nano ZnO and 2g of nano TiO2), ultrasonicate for 10min, reflux and stir at 82°C for 2h, centrifuge, wash the product with ethanol aqueous solution 4 times, and finally vacuum dry at 60°C, grind to obtain pretreated filler;

[0047] S5. Add 10g of pretreated filler and DMF into a three-necked flask with a stirring device. After mechanical stirring at room temperature for 1h, add 26.5g of anti-aging agent into the system and continue stirring for 30min. Then add 0.1g of EDC-HCl, transfer the mixture to a 60℃ water bath and continue stirring and reacting for 4h. After the reaction is completed, centrifuge and wash with ethanol aqueous solution for 5 times. Finally, dry the product in a vacuum oven at 60℃ and grind it to obtain a composite anti-aging agent.

[0048] Example 3

[0049] Preparation of aging-resistant silicone tube:

[0050] The first step is to add 1 kg of silicone rubber, 300 g of white carbon black, 60 g of phenyl silicone oil and 40 g of methyl silicone resin into a vacuum kneader, mix them evenly at room temperature, and then evacuate at 180°C for 2 hours to make a silicone rubber compound;

[0051] Step 2: Add 110 g of the composite antioxidant prepared in Example 1 to the silicone rubber mix, then mix evenly in a vacuum kneader, then add 20 g of 2,4-dichlorobenzoyl peroxide, and mix evenly on an open mill;

[0052] The third step is to cut the mixed rubber into small strips and extrude them on an extruder, and then vulcanize and shape them in a hot air drying tunnel or in a molding device to make a silicone tube.

[0053] Example 4

[0054] Preparation of aging-resistant silicone tube:

[0055] The first step is to add 1 kg of silicone rubber, 350 g of white carbon black, 75 g of phenyl silicone oil and 55 g of methyl silicone resin into a vacuum kneader, mix them evenly at room temperature, and then evacuate at 180°C for 2.5 hours to make a silicone rubber compound;

[0056] Step 2: Add 130 g of the composite antioxidant prepared in Example 2 to the silicone rubber mix, then mix evenly in a vacuum kneader, then add 25 g of di-tert-butyl peroxide, and mix evenly on an open mill;

[0057] The third step is to cut the mixed rubber into small strips and extrude them on an extruder, and then vulcanize and shape them in a hot air drying tunnel or in a molding device to make a silicone tube.

[0058] Example 5

[0059] Preparation of aging-resistant silicone tube:

[0060] The first step is to add 1 kg of silicone rubber, 400 g of white carbon black, 90 g of phenyl silicone oil and 70 g of methyl silicone resin into a vacuum kneader, mix them evenly at room temperature, and then evacuate at 180°C for 3 hours to make a silicone rubber compound;

[0061] Step 2: Add 150 g of the composite antioxidant prepared in Example 1 to the silicone rubber mix, then mix evenly in a vacuum kneader, then add 30 g of 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane), and mix evenly on an open mill;

[0062] The third step is to cut the mixed rubber into small strips and extrude them on an extruder, and then vulcanize and shape them in a hot air drying tunnel or in a molding device to make a silicone tube.

[0063] Comparative Example

[0064] The composite antioxidant in Example 3 is replaced with a mixture of nano ZnO and TiO2 and antioxidant 4010NA of equal mass, and the other raw materials and preparation process remain unchanged to obtain a silicone tube.

[0065] The following performance tests were performed on the silicone tubes obtained in Examples 3-5 and Comparative Examples:

[0066] UV aging resistance: UV aging test is carried out in QUV UV accelerated aging tester according to GB / T 14522-2008 standard;

[0067] Mechanical properties: Test the hardness and tensile properties of samples before and after aging in accordance with GB / T 531-1999 and GB / T 528-1998;

[0068] Flame retardant performance: Test the flame retardant performance of the sample in accordance with GB / T 10707-2008;

[0069] The measured results are shown in the following table:

[0070]

[0071] It can be seen from the data in the above table that the silicone rubber obtained in the present invention has high aging resistance and flame retardant properties; combined with the comparative data, it can be seen that in the present invention, by chemically compounding the organic light stabilizer on the surface of the inorganic anti-aging filler, the two components can promote each other, which can not only improve the anti-aging performance, but also promote dispersion, and will not have a negative impact on the mechanical properties of the silicone rubber.

[0072] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An aging-resistant silicone tube for ventilation and water circulation, characterized in that: The following raw materials are included in parts by weight: 100 parts of silicone rubber, 30-40 parts of white carbon black, 2-3 parts of vulcanizing agent, 6-9 parts of phenyl silicone oil, 11-15 parts of composite antioxidant, and 4-7 parts of methyl silicone resin; Wherein, the composite antioxidant is prepared by the following steps: S1. Add 5-nitroisophthalic acid and pentamethylpiperidinol to a three-necked flask, then add p-toluenesulfonic acid and toluene, and heat under constant stirring. Heat to reflux at 126-130° C. for 2.5 h, and then keep warm for 1 h. Cool the reaction solution, remove toluene by distillation under reduced pressure, and then wash the organic phase with saturated brine and saturated sodium carbonate solution for multiple times in sequence. Recrystallize the crude product with ethanol to obtain intermediate 1; add intermediate 1 and toluene to a reactor, add palladium carbon catalyst, remove air in the reactor under reduced pressure, and then introduce hydrogen. Perform reduction reaction under a pressure of 2 atm for 3 h. After completion, filter, and remove toluene from the filtrate by rotary distillation under reduced pressure to obtain intermediate 2; S2, add intermediate 2, triethylamine and benzene to a dry three-necked flask, place the flask in an ice bath, stir and mix, when the system temperature is stable at 0-2°C, slowly dropwise add a benzene solution of cyanuric chloride under stirring, react at 0-2°C for 3h after the dropwise addition is complete, filter to remove the generated salt, remove the solvent by vacuum rotary evaporation, purify by column chromatography, and spin-dry the eluent to obtain intermediate 3; S3, remove the air in the four-necked flask with N2, add 4-chlorobutyric acid and acetone, stir and mix evenly, place in an ice-water bath, slowly drop triethylamine and benzene solution of intermediate 3 while stirring, after the dropwise addition is complete, heat to 40°C and react for 4h, remove triethylamine hydrochloride by suction filtration, and obtain an anti-aging additive after the filtrate is distilled under reduced pressure; S4, treating the anti-aging filler with γ-aminopropyltriethoxysilane to obtain a pretreated filler; the anti-aging filler is a compound of nano ZnO and nano TiO2 in a mass ratio of 2:1-2; S5. Add the pretreated filler and DMF into a three-necked flask with a stirring device. After mechanical stirring at room temperature for 1 hour, add the anti-aging agent into the system and continue stirring for 30 minutes. Then add EDC-HCl, transfer the mixed solution to a 60°C water bath and continue stirring and reacting for 4 hours. After the reaction is completed, centrifuge and wash with ethanol aqueous solution for 4-5 times. Finally, dry the product in a vacuum oven at 60°C and grind it to obtain a composite anti-aging agent.

2. The aging-resistant silicone tube for ventilation and water flow according to claim 1, characterized in that: In step S1, the usage ratio of 5-nitroisophthalic acid, pentamethylpiperidinol, p-toluenesulfonic acid and toluene is 10.6 g:17.1 g:1.4 g:40 mL.

3. The aging-resistant silicone tube for ventilation and water circulation according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 2, triethylamine and cyanuric chloride used is 43.9 g:9.1 g:5.5 g.

4. The aging-resistant silicone tube for ventilation and water circulation according to claim 1, characterized in that: In step S3, the ratio of the amount of 4-chlorobutyric acid, intermediate 3 and triethylamine used is 6.2g:28.1g:5.1g.

5. The aging-resistant silicone tube for ventilation and water circulation according to claim 1, characterized in that: The specific operation of step S4 is as follows: γ-aminopropyltriethoxysilane and ethanol aqueous solution are added into a round-bottom flask, and after being mixed and dissolved evenly, an anti-aging filler is added, and after ultrasonication for 10 minutes, the reaction is refluxed and stirred at 82° C. for 2 hours, and centrifuged. The product is washed with ethanol aqueous solution for 3-4 times, and finally vacuum dried at 60° C. and ground to obtain a pretreated filler.

6. The aging-resistant silicone tube for ventilation and water circulation according to claim 1, characterized in that: In step S5, the ratio of the amount of the pretreated filler, the anti-aging aid and EDC-HCl is 10 g:26.5 g:0.1 g.

7. The method for preparing an aging-resistant silicone tube for ventilation and water permeation according to claim 1, characterized in that: The steps include: The first step is to add silicone rubber, white carbon black, phenyl silicone oil and methyl silicone resin into a vacuum kneader, mix them evenly at room temperature, and then evacuate at 180°C for 2-3 hours to make a silicone rubber compound; Step 2: Add the composite antioxidant to the silicone rubber compound, then mix it evenly in a vacuum kneader, then add the vulcanizing agent, and mix it evenly on an open mill; The third step is to cut the mixed rubber into small strips and extrude them on an extruder, and then vulcanize and shape them in a hot air drying tunnel or in a molding device to make a silicone tube.