A method for regulating the luminescence properties of quantum dots by surface ligands
By performing coordination equilibrium reaction and ultrafiltration dialysis in buffer solution, the luminescence properties of Ag2Se quantum dots are regulated, and the problems of quantum dot stability and composition structure are solved, and effective regulation and stability of the luminescence properties of quantum dots are achieved. Keep.
Patent Information
- Application Number
- CN202310291213.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-03-23
AI Technical Summary
The prior art is difficult to maintain the stability and compositional structure of quantum dots when regulating the luminescence properties of quantum dots, and ligand exchange after synthesis may lead to uneven aggregation, affecting optical and electronic properties.
By dispersing the quantum dots in a buffer solution for coordination equilibrium reaction, controlling the pH value and ligand structure, ensuring that the organic ligands are firmly bound to the surface of the quantum dots, regulating the energy level and emission wavelength of the Ag2Se quantum dots, and using ultrafiltration and dialysis The steps are used to maintain the purification and stability of the quantum dots.
Effective regulation of the luminescence properties of quantum dots is achieved, the stability and composition structure of quantum dots are maintained, and the emission wavelength and energy level are regulated to the maximum extent. It is suitable for Ag2Se quantum dots with different ligand densities.
Smart Images

Figure CN116333725B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of quantum dots, and in particular relates to a method for regulating the luminescence properties of quantum dots by surface ligands. Background Art
[0002] Quantum dots have attracted great attention in optoelectronic devices, photocatalysis, biosensing and biomedical imaging due to their excellent and adjustable optical and electronic properties. Quantum dots are composed of an inorganic core and a surface-bound ligand layer. The surface chemistry of quantum dots can regulate the optical absorption and photoluminescence properties, optoelectronic properties, and even electronic structure and energy band of quantum dots, which is a direct factor affecting the luminescence properties of quantum dots. Giansante and Frederick et al. reported that specific categories of ligands, such as short conjugated or aromatic molecules, can enhance the optical absorption of quantum dots in optoelectronic applications by changing the electronic state of quantum-ligand complexes. At the same time, Brown et al. found that the band gap energy of quantum dots can be changed by ligand exchange, and the energy level of PbS quantum dots can be changed by 0.9 eV by exchanging different types of ligands. At present, changing ligands during synthesis and ligand exchange after synthesis are the main means to explore the influence of ligands and regulate the properties of quantum dots. Studies have reported that the type of ligand or reaction concentration will affect the reactivity of precursors during synthesis and lead to the synthesis of quantum dots of different sizes and compositions. Ligand exchange after synthesis may lead to poor stability and uneven aggregation of quantum dots. Summary of the invention
[0003] In view of this, the present invention provides a method for regulating the luminescence properties of quantum dots by surface ligands. The method provided by the present invention can achieve the regulation of the luminescence properties of quantum dots while maintaining the original composition, structure and stability of the quantum dots.
[0004] In order to solve the above technical problems, the present invention provides a method for regulating the luminescence properties of quantum dots by surface ligands, which can achieve the regulation of the luminescence properties of quantum dots, comprising the following steps:
[0005] The quantum dots are dispersed in a buffer solution to carry out a coordination equilibrium reaction; the pH value of the buffer solution is 2.0 to 12.0; the average particle size of the quantum dots is 2.0±0.2 nm, and the quantum dots include an inorganic core and an organic ligand, the inorganic core is Ag2Se, and the organic ligand has a structure as shown in Formula 1:
[0006]
[0007] Wherein R is amino, pyridyl, imidazolyl or aniline.
[0008] Preferably, the buffer solution is a BR buffer solution.
[0009] Preferably, before the dispersing, the method further comprises: dispersing the quantum dots in ultrapure water and sequentially performing ultrafiltration and dialysis.
[0010] Preferably, the ultrafiltration comprises the following steps: performing a first ultrafiltration using an ultrafiltration tube with a molecular weight cutoff of 50 kDa to obtain quantum dots with a molecular weight less than 50 kDa; performing a second ultrafiltration using an ultrafiltration tube with a molecular weight cutoff of 10 kDa to obtain quantum dots with a molecular weight greater than 10 kDa and less than 50 kDa, and the second ultrafiltration is performed more than 30 times.
[0011] Preferably, the dialysis comprises the following steps: dialyzing the quantum dot solution obtained by ultrafiltration for more than 48 hours using a dialysis bag with a molecular weight cutoff of 3500Da, and changing the water every 8 hours during the dialysis process.
[0012] Preferably, the method further comprises freeze-drying the dialyzed quantum dots after the dialysis.
[0013] Preferably, when R is an amino group, the method for preparing the quantum dots comprises the following steps:
[0014] mixing a sodium hydroxide solution, a silver nitrate solution and alanine to obtain a silver precursor solution;
[0015] The sodium selenite solution, glutathione, reduced coenzyme II, glutathione reductase and BR buffer solution are mixed and reacted to obtain a selenium precursor solution;
[0016] A silver precursor solution and a selenium precursor solution are mixed under a protective atmosphere to synthesize quantum dots, thereby obtaining Ag2Se quantum dots in which R is an amino group; the molar ratio of silver nitrate to sodium selenite in the silver nitrate solution is 6:1.
[0017] Preferably, the temperature of the mixed reaction is 19 to 21° C., and the time of the mixed reaction is 10 to 40 seconds;
[0018] The temperature for synthesizing the quantum dots is 90° C., and the time for synthesizing the quantum dots is 10 s.
[0019] The present invention provides a method for regulating the luminescence properties of quantum dots by surface ligands, comprising the following steps: dispersing quantum dots in a buffer solution to perform a coordination equilibrium reaction; the pH value of the buffer solution is 2.0 to 12.0; the average particle size of the quantum dots is 2.0±0.2 nm, the quantum dots include an inorganic core and an organic ligand, the inorganic core is Ag2Se, and the organic ligand has a structure as shown in Formula 1: Wherein R is amino, pyridyl, imidazole or aniline. The present invention disperses the thiol-coordinated quantum dots in buffer solutions of different pH values to form double-coordinated quantum dots after coordination equilibrium reaction. In the present invention, when R is amino, the pH value of the buffer solution is 7.0-12.0, when R is pyridyl, the pH value of the buffer solution is 2.0-7.0, when R is imidazole, the pH value of the buffer solution is 3.0-7.0, and when R is aniline, the pH value of the buffer solution is 3.0-9.0. The quantum dots whose surface ligand is glutathione are dispersed in a buffer solution with a pH value of 2.0-12.0, and the coordination of the amino group on glutathione will cause the surface ligand of the quantum dots to gradually form a thiol-amino double-coordinated binding state. When the surface of quantum dots is regulated by the present invention, the organic ligands on the surface of quantum dots can be firmly bound to the surface of quantum dots. By in-situ regulating the binding state of the surface nitrogen-containing groups R and the silver ions on the surface of the inorganic core, the energy level of the Ag2Se quantum dots can be regulated up to 140 meV, and the emission wavelength can be regulated up to 75 nm. The method provided by the present invention is applicable to Ag2Se quantum dots with different ligand densities on the surface of quantum dots. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The fluorescence performance comparison spectra of the dried Ag2Se quantum dots prepared in Example 1 after being regulated by buffer solutions with different pH values are shown in FIG.
[0021] Figure 2 TEM image of the purified Ag2Se quantum dots prepared in Example 1;
[0022] Figure 3 XRD spectrum of the purified Ag2Se quantum dots prepared in Example 1;
[0023] Figure 4 This is the X-ray photoelectron spectrum of the purified Ag2Se quantum dots prepared in Example 1;
[0024] Figure 5 This is the hydrated particle size distribution diagram of the purified Ag2Se quantum dots prepared in Example 1;
[0025] Figure 6 The purified and freeze-dried Ag2Se quantum dots prepared in Example 1 were dispersed in D2O. 1 H NMR spectrum;
[0026] Figure 7 The purified lyophilized Ag2Se quantum dots prepared in Example 1 were prepared in different solvents (D2O and NaOD) 1 H NMR spectrum;
[0027] Figure 8Schematic diagram of the change of the coordination state of the amino group in the quantum dots during the regulation process in Example 1;
[0028] Fig. 9 The fluorescence spectra of the purified and freeze-dried Ag2Se quantum dots with different surface ligand densities prepared in Examples 1 to 4 in buffer solutions ranging from pH 7.0 to pH 12.0;
[0029] Fig.10 This is a fluorescence spectrum of the quantum dots with pyridyl as the R group prepared in Example 5 in a buffer solution of pH 2.0 to pH 7.0. DETAILED DESCRIPTION
[0030] The present invention provides a method for regulating the luminescence properties of quantum dots by surface ligands, comprising the following steps:
[0031] Dispersing the quantum dots in a buffer solution to carry out a coordination equilibrium reaction; the pH value of the buffer solution is 2.0 to 12.0;
[0032] The average particle size of the quantum dots is 2.0±0.2 nm. The quantum dots include an inorganic core and an organic ligand. The inorganic core is Ag2Se, and the organic ligand has a structure as shown in Formula 1:
[0033]
[0034] Wherein R is amino, pyridyl, imidazole or aniline, preferably amino. In the present invention, R is a pH sensitive group. In the present invention, the average particle size of the quantum dots is preferably 2 nm.
[0035] In the present invention, the buffer solution is preferably a BR buffer solution. In the present invention, the BR buffer solution is preferably prepared according to the following method:
[0036] first mixing the phosphoric acid solution, the boric acid solution and the acetic acid solution to obtain an acidic mixed solution;
[0037] The acidic mixed solution and the sodium hydroxide solution are mixed for a second time, and the pH value is adjusted to obtain the BR buffer solution.
[0038] In the present invention, the molar concentration of the phosphoric acid solution is preferably 0.04 mol / L, the molar concentration of the boric acid solution is preferably 0.04 mol / L, and the molar concentration of the acetic acid solution is preferably 0.04 mol / L. The present invention has no special requirements for the first mixing, as long as it can be mixed evenly.
[0039] In the present invention, the molar concentration of the sodium hydroxide solution is preferably 0.2 mol / L. The present invention has no special limitation on the amount of the sodium hydroxide solution, as long as the required pH value can be met. The present invention has no special requirements for the second mixing, as long as it can be mixed evenly.
[0040] In the present invention, the pH value of the buffer solution is preferably based on the pK a The pH value is determined. In the present invention, when R is an amino group, the pH value of the buffer solution is 7.0-12.0, when R is a pyridyl group, the pH value of the buffer solution is 2.0-7.0, when R is an imidazole group, the pH value of the buffer solution is 3.0-7.0, and when R is an aniline group, the pH value of the buffer solution is 3.0-9.0.
[0041] In the present invention, when R is an amino group, the method for preparing the quantum dots preferably comprises the following steps:
[0042] mixing a sodium hydroxide solution, a silver nitrate solution and alanine to obtain a silver precursor solution;
[0043] The sodium selenite solution, glutathione, reduced coenzyme II, glutathione reductase and BR buffer solution are mixed and reacted to obtain a selenium precursor solution;
[0044] A silver precursor solution and a selenium precursor solution are mixed under a protective atmosphere to synthesize quantum dots to obtain Ag2Se quantum dots in which R is an amino group; the molar ratio of the silver nitrate in the silver nitrate solution to the sodium selenite in the sodium selenite solution is 6:1.
[0045] Sodium hydroxide solution, silver nitrate solution and alanine (L-Ala) are mixed to obtain a silver precursor solution. In the present invention, the molar concentration of the sodium hydroxide solution is preferably 0.1 mol / L, the molar concentration of the silver nitrate is preferably 0.1 mol / L, the volume ratio of the sodium hydroxide solution to the silver nitrate solution is preferably 93:1, and the molar ratio of silver nitrate to alanine in the silver nitrate solution is preferably 1:1.25. The present invention preferably performs mixing under deoxygenation conditions, and the deoxygenation is preferably performed by passing argon into the mixed solution. In the present invention, the mixing is preferably performed under stirring conditions, and the present invention has no special requirements for the stirring, as long as it can be mixed evenly.
[0046] Sodium selenite (Na2SeO3) solution, glutathione, reduced coenzyme II (NADPH), glutathione reductase and BR buffer solution are mixed to react to obtain a selenium precursor solution. In the present invention, the molar concentration of the sodium selenite solution is preferably 0.1 mol / L, the molar ratio of sodium selenite to glutathione in the sodium selenite solution is preferably 1:4, the molar ratio of glutathione to NADPH is preferably 4:1, and the volume ratio of the mole of glutathione to glutathione reductase is preferably 1 μmol:1~1.1 μL, more preferably 1 μmol:1 μL. In the present invention, the volume ratio of the BR buffer solution to the volume ratio of the sodium hydroxide solution is preferably 1:1, and the pH value of the BR buffer solution is preferably 7.1. In the present invention, the temperature of the mixed reaction (reaction to generate a selenium precursor) is preferably 19~21°C, more preferably 20°C, and the time of the mixed reaction (reaction to generate a selenium precursor) is preferably 10~40s, more preferably 20s. In the present invention, the mixed reaction process includes two processes: sodium selenite is reduced to generate seleno-oxidized glutathione derivatives (GSSeSG) and GSSeSG is reduced to generate seleno-reduced glutathione derivatives (GSSeH). In the present invention, the mixed reaction is preferably carried out under stirring conditions, and the present invention has no special requirements for the stirring, as long as it can be mixed evenly.
[0047] After obtaining the silver precursor solution and the selenium precursor solution, the present invention mixes the silver precursor solution and the selenium precursor solution under a protective atmosphere to synthesize quantum dots, and obtains Ag2Se quantum dots in which R is an amino group. In the present invention, the temperature for synthesizing the quantum dots is preferably 90° C., and the time for synthesizing the quantum dots is preferably 10 seconds. The present invention controls the density of the ligands on the surface of the quantum dots by controlling the time of the mixing reaction (generating the selenium precursor reaction).
[0048] The present invention preferably cools the system after the quantum dot synthesis, and the present invention has no special requirements for the cooling method.
[0049] In the present invention, when R is a pyridyl group, an imidazole group or an aniline group, the method for preparing the quantum dots preferably comprises the following steps:
[0050] The prepared quantum dots whose R is an amino group are dispersed in a BR buffer solution with a pH value of 8 after ultrafiltration, and then mixed with a substance containing a pyridine group, an imidazole group or an aniline group for a condensation reaction to obtain Ag2Se quantum dots whose R is a pyridine group, an imidazole group or an aniline group.
[0051] Taking R as pyridyl as an example, the preparation method is as follows: 5 mg of the prepared quantum dots in which R is amino group are subjected to a first ultrafiltration using an ultrafiltration tube with a molecular weight cutoff of 50 kDa to obtain quantum dots with a molecular weight less than 50 kDa; a second ultrafiltration is performed using an ultrafiltration tube with a molecular weight cutoff of 10 kDa to obtain quantum dots with a molecular weight greater than 10 kDa and less than 50 kDa, which are dispersed in a BR buffer solution with a pH value of 8 and then mixed with 3 mg of isonicotinic acid for a condensation reaction (accompanied by stirring for 12 hours at room temperature) to obtain Ag2Se quantum dots in which R is pyridyl.
[0052] In the present invention, the dispersion preferably further includes: dispersing the quantum dots in ultrapure water and performing ultrafiltration and dialysis in sequence. In the present invention, the ultrafiltration preferably includes the following steps: using an ultrafiltration tube with a molecular weight cutoff of 50kDa to perform a first ultrafiltration to obtain quantum dots with a molecular weight less than 50kDa; using an ultrafiltration tube with a molecular weight cutoff of 10kDa to perform a second ultrafiltration to obtain quantum dots with a molecular weight greater than 10kDa and less than 50kDa, and the number of the second ultrafiltration is more than 30 times. In the present invention, the dialysis preferably includes the following steps: using a dialysis bag with a molecular weight cutoff of 3500Da to dialyze the quantum dot solution obtained by ultrafiltration for more than 48 hours, and changing the water every 8 hours during the dialysis process.
[0053] In the present invention, the quantum dots obtained by dialysis are preferably freeze-dried and then stored.
[0054] The present invention has no special requirements for the dispersion, as long as it can be dispersed evenly.
[0055] In the present invention, the temperature of the coordination equilibrium reaction is preferably room temperature, more preferably 30° C. The present invention preferably detects the endpoint of the coordination equilibrium reaction by the luminescence performance of quantum dots, specifically by using a fluorescence spectrometer to detect the fluorescence spectrum of the quantum dot dispersion before the coordination equilibrium reaction. When the fluorescence peak position of the quantum dots no longer moves, it indicates that the coordination equilibrium reaction is over.
[0056] The Ag2Se quantum dots prepared by the control method provided by the present invention have a large specific surface area and are silver-rich on the surface. + The thiol group has strong binding ability. During the regulation process, the thiol group on the ligand can always bind to the surface Ag. + The ligand is bound to the surface of the quantum dot so that the ligand does not leave the surface. The ligand contains another pH-sensitive group and is + The bound group makes the binding state of the ligand controlled by the pH value of the solution. By controlling the pH value, the binding state of the ligand can be regulated, thereby regulating the fluorescence properties of the quantum dots.
[0057] The control method used in the present invention controls the coordination state of the surface group while ensuring that the ligand does not leave the surface, and can control the fluorescence emission wavelength and energy level to the maximum extent without destroying the precursor of the quantum dot structure. It provides a new way for in-depth research on surface chemistry and control of the properties of quantum dots, and lays a foundation for the construction of functional materials based on quantum dots.
[0058] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0059] Example 1
[0060] 18.5 mL of a freshly prepared NaOH solution with a molar concentration of 0.1 mol / L was placed in a 50 mL three-necked flask, and high-purity argon was introduced for deoxygenation for 15 min, and then 198 μL of a freshly prepared AgNO3 (19.8 μmol) solution with a molar concentration of 0.1 mol / L and 2.2 mg of L-Ala (24.7 μmol) were added, and the mixture was mixed and stirred to obtain a Ag precursor solution;
[0061] 18.5 mL of BR buffer solution with a pH value of 7.1 was placed in a 25 mL two-necked flask, the water bath temperature was adjusted to 20°C, argon was introduced for 15 min, and then 4.06 mg of GSH (13.2 μmol), 33 μL of sodium selenite solution with a molar concentration of 0.1 mol / L Na2SeO3 (3.3 μmol), 2.75 mg of NADPH (3.3 μmol) and glutathione reductase (13.3 μL) were added to the flask in sequence, and a mixing reaction was carried out at 20°C for 20 s (with stirring), and the Se precursor solution was obtained when the color of the solution changed from colorless to light yellow.
[0062] The Se precursor solution was placed in an argon environment at 90°C for 20 seconds and then injected into the Ag precursor solution. The quantum dots were synthesized for 10 seconds and then taken out and quickly cooled on ice to obtain Ag2Se quantum dots.
[0063] After dispersing the Ag2Se quantum dots in ultrapure water, first purify the solution with a molecular weight less than 50kDa using an ultrafiltration tube with a molecular weight cutoff of 50kDa, and then ultrafilter and purify at least 30 times using an ultrafiltration tube with a molecular weight cutoff of 10kDa, and retain the solution with a molecular weight greater than 10kDa; use a dialysis bag with a molecular weight cutoff of 3500Da to dialyze the quantum dot solution with a molecular weight greater than 10kDa and less than 50kDa retained by ultrafiltration for more than 48 hours, and change the water every 8 hours during the dialysis process; freeze-dry the dialyzed quantum dot solution for standby use to obtain purified freeze-dried Ag2Se quantum dots;
[0064] 1 mg of purified lyophilized Ag2Se quantum dots were dispersed in 2 mL of BR buffer solutions with pH values of 7.0, 8.0, 9.0, 10.0, 11.0 and 12.0 to regulate the fluorescence properties of the quantum dots and obtain quantum dot dispersions with different pH values; 500 μL of dispersions with different pH values were taken in micro quartz cuvettes, and the fluorescence properties were detected on a fluorescence spectrophotometer (excitation wavelength of 490 nm, scanning the emission range of 600-900 nm); the obtained fluorescence spectra were normalized to obtain Figure 1 .Depend on Figure 1 It can be seen that as the pH value of the dispersion used in the regulation process increases, the fluorescence spectrum of the quantum dots gradually blue-shifts and the fluorescence intensity gradually increases.
[0065] The properties of the purified and freeze-dried Ag2Se quantum dots were characterized, and TEM images, XRD spectra, X-ray photoelectron spectroscopy and hydrated particle size distribution were obtained, such as Figures 2 to 5 As shown, Figure 2 For TEM images, Figure 3 is the XRD spectrum, Figure 4 is the X-ray photoelectron spectrum, Figure 5 is the hydrated particle size distribution diagram. Figure 2 and Figure 5 It can be seen that the obtained quantum dots are Ag2Se quantum dots with a particle size of 2nm and a hydrated particle size of 2.7nm. Figure 3 and Figure 4 It can be seen that the quantum dots prepared in the embodiment of the present invention are Ag2Se quantum dots, which match the spectrum of Ag2Se.
[0066] Quantitative nuclear magnetic resonance analysis showed that the number of glutathione on the surface of dried Ag2Se quantum dots was 35, and the fluorescence emission peak was 750nm.
[0067] Purified freeze-dried Ag2Se quantum dots were dispersed in D2O 1 H NMR detection (scanning time is 30 min) 1 H NMR spectrum, such as Figure 6 shown. Figure 6 The results showed that the surface ligand of quantum dots was glutathione. The prepared dried Ag2Se quantum dots were dispersed in different solvents (D2O, NaOD solution with a molar concentration of 0.01 mol / L) and then subjected to NMR measurement. 1 H NMR spectrum, such as Figure 7 As shown. Figure 7 It can be seen that the amino groups on the surface of the quantum dots are deprotonated and then bound to the surface of the quantum dots. The schematic diagram of the binding process after deprotonation is shown in Figure 8 shown.
[0068] Example 2
[0069] Dry Ag2Se quantum dots were prepared according to the method of Example 1, except that the mixing reaction time was 10 s.
[0070] Quantitative nuclear magnetic resonance analysis showed that the number of glutathione on the surface of dried Ag2Se quantum dots was 17, and the fluorescence emission peak was 740nm.
[0071] Example 3
[0072] Dry Ag2Se quantum dots were prepared according to the method of Example 1, except that the mixing reaction time was 30 s.
[0073] Quantitative nuclear magnetic resonance analysis showed that the number of glutathione on the surface of dried Ag2Se quantum dots was 44, and the fluorescence emission peak was 760nm.
[0074] Example 4
[0075] Dry Ag2Se quantum dots were prepared according to the method of Example 1, except that the mixing reaction time was 40 s.
[0076] Quantitative nuclear magnetic resonance analysis showed that the number of glutathione on the surface of dried Ag2Se quantum dots was 50, and the fluorescence emission peak was 770nm.
[0077] The surface ligands of the Ag2Se quantum dots prepared in Examples 1 to 4 were quantitatively detected by nuclear magnetic resonance quantitative determination, and the number of surface ligands per quantum dot was 35, 17, 44 and 50, respectively, and the surface ligand density was 2.8 nm, respectively. -2 , 1.4nm -2 、3.5nm -2 and 4.0nm -2 The Ag2Se quantum dots prepared in Examples 1 to 4 were dispersed in BR buffer solutions with pH values of 7.0, 8.0, 9.0, 10.0, 11.0 and 12.0, respectively, to obtain quantum dot dispersions with different pH values; 500 μL of the dispersions with different pH values were taken in micro quartz cuvettes, and the fluorescence properties were detected on a fluorescence spectrophotometer (excitation wavelength of 490 nm, scanning the emission range of 600 to 900 nm). The fluorescence spectrum is shown in the figure below. Fig. 9 As shown, according to Fig. 9 It can be seen that the fluorescence spectra of Ag2Se quantum dots with different surface ligand densities have similar pH response processes.
[0078] Example 5
[0079] Purified and freeze-dried Ag2Se quantum dots were prepared according to the method of Example 1;
[0080] 5 mg of dried Ag2Se quantum dots were dispersed in a BR buffer solution with a pH value of 8.0, 3 mg of isonicotinic acid was added, and stirred at room temperature for 12 h. The pH of the solution was monitored several times during the reaction to stabilize it at 8.0. Then, Ag2Se@PY quantum dots were purified using a 10 kDa ultrafiltration tube and freeze-dried for later use.
[0081] 1 mg of dried Ag2Se@PY quantum dots were dispersed in 2 mL of BR buffer solution with pH values of 2.0, 3.0, 4.0, 5.0, 6.0 and 7.0 to obtain Ag2Se@PY dispersions with different pH values; 500 μL of dispersions with different pH values were taken in micro quartz cuvettes and the fluorescence properties were detected on a fluorescence spectrophotometer. The fluorescence spectra are shown in the figure below. Fig.10 As shown. Fig.10 It can be seen that the fluorescence spectrum of quantum dots will also be regulated by pH after the surface amino groups are replaced by pyridine groups.
[0082] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for regulating the luminescence properties of quantum dots by surface ligands, which can achieve the regulation of the luminescence properties of quantum dots, comprising the following steps: The quantum dots are dispersed in a buffer solution to carry out a coordination equilibrium reaction; The pH value of the buffer solution is 2.0-12.0; the buffer solution is a BR buffer solution; the average particle size of the quantum dots is 2.0±0.2 nm, and the quantum dots include an inorganic core and an organic ligand, the inorganic core is Ag2Se, and the organic ligand has a structure as shown in Formula 1: Formula 1; Wherein R is amino or pyridyl; Before the dispersion, the method further comprises: dispersing the quantum dots in ultrapure water and sequentially performing ultrafiltration and dialysis; When R is an amino group, the method for preparing the quantum dots comprises the following steps: mixing a sodium hydroxide solution, a silver nitrate solution and alanine to obtain a silver precursor solution; The sodium selenite solution, glutathione, reduced coenzyme II, glutathione reductase and BR buffer solution are mixed and reacted to obtain a selenium precursor solution; A silver precursor solution and a selenium precursor solution are mixed under a protective atmosphere to synthesize quantum dots to obtain Ag2Se quantum dots in which R is an amino group; the molar ratio of silver nitrate to sodium selenite in the silver nitrate solution is 6:1; When R is a pyridyl group, the preparation method of the quantum dots is as follows: using an ultrafiltration tube with a molecular weight cutoff of 50kDa to perform a first ultrafiltration on 5 mg of the prepared quantum dots in which R is an amino group to obtain quantum dots with a molecular weight less than 50kDa; using an ultrafiltration tube with a molecular weight cutoff of 10kDa to perform a second ultrafiltration to obtain quantum dots with a molecular weight greater than 10kDa and less than 50kDa, dispersing them in a BR buffer solution with a pH value of 8, and mixing them with 3mg of isonicotinic acid for a condensation reaction to obtain Ag2Se quantum dots in which R is a pyridyl group.
2. The method according to claim 1, characterized in that: The ultrafiltration comprises the following steps: performing a first ultrafiltration using an ultrafiltration tube with a molecular weight cutoff of 50 kDa to obtain quantum dots with a molecular weight less than 50 kDa; performing a second ultrafiltration using an ultrafiltration tube with a molecular weight cutoff of 10 kDa to obtain quantum dots with a molecular weight greater than 10 kDa and less than 50 kDa, wherein the second ultrafiltration is performed for more than 30 times.
3. The method according to claim 1, characterized in that: The dialysis comprises the following steps: dialyzing the quantum dot solution obtained by ultrafiltration for more than 48 hours using a dialysis bag with a molecular weight cutoff of 3500Da, and changing the water every 8 hours during the dialysis process.
4. The method according to claim 1, 2 or 3, characterized in that: After the dialysis, the method further comprises: freeze-drying the dialyzed quantum dots.
5. The method according to claim 1, characterized in that: The temperature of the mixed reaction is 19-21°C, and the time of the mixed reaction is 10-40s; The temperature for synthesizing the quantum dots is 90° C., and the time for synthesizing the quantum dots is 10 s.