Preparation method of flame retardant material based on graphene oxide

Through the layer-by-layer self-assembly method of modified graphene oxide solution, the problem of uneven distribution of graphene oxide in flame-retardant materials is solved, the flame-retardant performance and preparation efficiency are improved, and efficient preparation of graphene oxide flame-retardant materials is achieved. .

CN116334913BActive Publication Date: 2024-10-25WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310210008.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-10-25
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

The existing graphene oxide is unevenly distributed during the layer-by-layer self-assembly process, which affects its flame retardant performance. The preparation process is cumbersome and requires multiple assembly and high loading.

Method used

Using a layer-by-layer self-assembly method, the adhesive spreading solution, graphene oxide solution and phytic acid solution are assembled on the substrate through dendritic polyethyleneimine aqueous solution, enzymatic nanocellulose and tannic acid-modified graphene oxide solution. Ensures even distribution and high compatibility.

Benefits of technology

The compatibility and adhesion between graphene oxide and the substrate are improved, the usage of graphene oxide is reduced, the preparation process is simplified, the flame retardant performance and preparation efficiency are improved, and the limiting oxygen index reaches 30.6-32.2. Smoke emission is reduced by 60%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116334913B_ABST
    Figure CN116334913B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a flame retardant material based on graphene oxide, wherein a graphene oxide solution with good ductility is prepared by first dispersing graphene oxide using enzymatic nanocellulose and then adding tannic acid to change the aggregation tendency of graphene oxide, and then a layer-by-layer self-assembly method is used to sequentially assemble an adhesive spreading liquid, a graphene oxide solution, and a phytic acid solution on a substrate. In the above process, by controlling the mass percentage of enzymatic nanocellulose, graphene oxide, and tannic acid in the graphene oxide solution, the uniformity of the graphene oxide solution and its compatibility with the substrate are effectively improved, ensuring the adhesion between the graphene oxide solution and the substrate and each coating during the layer-by-layer self-assembly process. In the above manner, a flame retardant material based on graphene oxide with uniform coating and excellent flame retardant properties is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant and smoke suppression fabrics, and in particular to a method for preparing a flame retardant material based on graphene oxide. Background Art

[0002] Graphene oxide is used as a flame retardant due to its unique two-dimensional structure and large specific surface area. It can improve the thermal stability of polymers and delay the combustion of polymers. Graphene oxide is a dark green powder derivative obtained from graphite through a series of oxidation and ultrasonic exfoliation methods. Its structure is a single-layer flaky crystal with a six-membered ring network structure arranged by carbon atoms. It has a large specific surface area and a large π conjugated structure. Both sides of the flaky layer can be combined with metals, non-metals, polymers, etc. through covalent and non-covalent interactions, so it has a very high loading capacity.

[0003] At present, graphene oxide is applied in the field of flame retardancy, mainly by preparing it into films or aerogels, or using it as an additive to improve the flame retardant properties of the target material. In order to improve the functionality of the material and the compatibility between graphene and the material, this method mostly achieves the goal by modifying graphene oxide. At the same time, due to the strong van der Waals force between graphene oxide sheets, it has a strong tendency to aggregate during the layer-by-layer self-assembly process as the solvent is removed during drying, resulting in uneven distribution of graphene oxide on the surface of the assembled flame retardant material, affecting the application of graphene oxide in layer-by-layer self-assembly flame retardancy. In addition, the layer-by-layer self-assembly flame retardant modification process usually has a lot of finishing steps, and the number of assembly layers required to achieve the ideal flame retardant effect is large, and the flame retardant load requirement is large.

[0004] In the prior art, the patent document entitled "Graphene oxide hybrid flame retardant and preparation method thereof" with application number CN201710357151.6 and publication number August 20, 2019, prepares a bisphenol acid-based polyphosphate electrolyte through a series of reactions, uses polyethyleneimine to graft graphene oxide, and then prepares graphene oxide hybrid flame retardant by electrostatic action of ammonium polyphosphate, polyethyleneimine, bisphenol acid-based polyphosphate electrolyte and modified graphene oxide. Although the graphene sheets in the graphene oxide hybrid flame retardant prepared by the above method have a good dispersion effect, the realization of this purpose depends on the design of a specific molecular structure, and the preparation process of the required substances is cumbersome, and the flame retardant effect needs to be improved.

[0005] In the prior art, in the patent document entitled "A flame retardant coating and its preparation method and application" with application number CN201210378384.1 and publication number December 3, 2014, a phosphorus-nitrogen flame retardant is prepared by first using diethyl chlorophosphate and acrylamine or acrylamine hydrochloride to react under specific conditions, and then reacting it with acrylamine monomer under the conditions of initiation by an initiator to obtain flame retardant modified polyacrylamine, and further preparing flame retardant polyester cotton fiber. In the above process, the synergistic effect between the intumescent flame retardant and graphene oxide is mainly used to improve the flame retardant properties of the material; however, in the above technical solution, when obtaining the flame retardant polyester cotton fiber, the polyester cotton fiber needs to be repeatedly immersed in the modified polyacrylamine aqueous solution and the graphene oxide suspension, and the flame retardant is continuously assembled on the surface of the polyester cotton fiber, and the number of repetitions is up to 20 times. The process is cumbersome to operate, and it is not easy to ensure that the flame retardant is evenly assembled on the surface of the polyester cotton fiber.

[0006] In view of this, it is necessary to design an improved method for preparing a flame retardant material based on graphene oxide to solve the above problems. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a flame retardant material based on graphene oxide.

[0008] To achieve the above-mentioned purpose of the invention, the present invention provides a method for preparing a flame retardant material based on graphene oxide, wherein the flame retardant material is prepared by adopting a layer-by-layer self-assembly method to sequentially assemble an adhesive spreading liquid, a graphene oxide solution and a phytic acid solution on a substrate; the adhesive spreading liquid is an aqueous solution of dendritic polyethyleneimine, and the graphene oxide solution contains enzymatic nanocellulose, graphene oxide and tannic acid.

[0009] Furthermore, the method for preparing the flame retardant material based on graphene oxide comprises the following steps:

[0010] S1, preparing the branched polyethyleneimine aqueous solution, the phytic acid solution and the graphene oxide solution;

[0011] S2, soaking the substrate in the aqueous solution of dendritic polyethyleneimine obtained in step S1 for 1-30 minutes, taking it out and washing it to obtain a substrate assembled with the adhesive spreading solution;

[0012] S3, soaking the substrate assembled with the adhesive spreading liquid in step S2 in the pre-prepared graphene oxide solution and the phytic acid solution in sequence, and then drying, to obtain a flame retardant material based on graphene oxide.

[0013] Preferably, in step S1, the preparation of the graphene oxide solution comprises the following steps:

[0014] (1) dissolving enzymatically processed nanocellulose in water and dispersing the nanocellulose uniformly to obtain an enzymatically processed nanocellulose solution; dissolving graphene oxide in water and dispersing the nanocellulose uniformly to obtain a graphene oxide solution;

[0015] (2) Under continuous stirring, the graphene oxide solution prepared in step S1 is slowly poured into the enzymatic nanocellulose solution, and mixed evenly to obtain a mixed solution; then, tannic acid powder is added to the mixed solution, and mixed evenly to obtain the graphene oxide solution.

[0016] Preferably, the mass percentage of the enzymatic nanocellulose in the graphene oxide solution is 0.1-0.4%, the mass percentage of the graphene oxide is 0.25-1%, and the mass percentage of the tannic acid is 0.05-0.1%.

[0017] Preferably, in step S1, the mass percentage of the dendritic polyethyleneimine in the dendritic polyethyleneimine aqueous solution is 1-2%, and the mass percentage of the phytic acid solution is 0.5-1.0%.

[0018] Preferably, in step S3, the bath ratio of the substrate to the graphene oxide solution is 1:(50-100), and the bath ratio of the substrate to the phytic acid solution is 1:(50-100).

[0019] Preferably, in step S2, the bath ratio of the substrate to the aqueous solution of dendritic polyethyleneimine is 1:(20-80).

[0020] Preferably, in step S2, the substrate is further subjected to alkali treatment before being immersed in the branched polyethyleneimine aqueous solution. The alkali treatment is performed using a sodium hydroxide solution with a mass percentage of 2-4%. The temperature of the alkali treatment is 60° C. and the time is 60 min.

[0021] Preferably, in step S3, the immersion time of the substrate in the graphene oxide solution and the phytic acid solution is 1-30 min.

[0022] Preferably, the types of the substrate include woven fabrics, knitted fabrics, nonwoven fabrics, polyurethane foam, wood, and aerogel, and the types of fabric fibers include cotton, wool, silk, linen, polyester, viscose, and nylon.

[0023] The beneficial effects of the present invention are:

[0024] 1. The preparation method of the flame retardant material based on graphene oxide provided by the present invention is to obtain a graphene oxide solution with good ductility by first dispersing graphene oxide with enzymatic nanocellulose and then adding tannic acid to change the aggregation tendency of graphene oxide, and then assemble the adhesive spreading liquid, graphene oxide solution and phytic acid solution on the substrate in sequence by layer-by-layer self-assembly method. In the above process, by controlling the mass percentage of enzymatic nanocellulose, graphene oxide and tannic acid in the graphene oxide solution, it is ensured that the graphene oxide in the obtained graphene oxide solution is evenly distributed, and the compatibility between the graphene oxide solution and the substrate is effectively improved, and the adhesion between the graphene oxide solution and the substrate during the layer-by-layer self-assembly process is ensured; at the same time, by regulating the ratio of the adhesive spreading liquid, graphene oxide solution and phytic acid solution during the layer-by-layer self-assembly process, it is ensured that each layer is evenly distributed on the surface of the substrate and the layers are firmly bonded. In the above manner, a flame retardant material based on graphene oxide with excellent flame retardancy is obtained.

[0025] 2. The preparation method of the flame retardant material based on graphene oxide provided by the present invention, by using enzymatic nanocellulose to disperse graphene oxide in the process of preparing graphene oxide solution, and introducing tannic acid to change the aggregation tendency of graphene oxide, avoiding the aggregation between graphene oxide as the solvent molecules evaporate during the layer-by-layer self-assembly process, and making the graphene oxide coating on the surface of the substrate unevenly distributed and affecting the flame retardancy of the flame retardant, maximizing the flame retardancy of graphene oxide, and reducing the amount of graphene oxide used in the preparation process of flame retardant materials; by assembling the adhesive spreading liquid, graphene oxide solution and phytic acid solution on the substrate successively, the dendritic polyethyleneimine can be used to charge the surface of the substrate, increasing the interaction between the substrate and each coating when the graphene oxide and phytic acid are subsequently assembled, and thus the preparation method proposed by the present invention is adopted, and only a single cycle is required to obtain a flame retardant material with excellent flame retardant performance, which effectively improves the preparation efficiency of the flame retardant material. In particular, the mass percentages of enzymatic nanocellulose, graphene oxide and phytic acid in the preparation process of the present invention are all less than 1%, which has the advantages of less materials and simple materials. By adopting the method for preparing a flame retardant material based on graphene oxide proposed in the present invention, the flame retardant material prepared can have a limiting oxygen index of 30.6 at a minimum weight gain of 8.9%, and its limiting oxygen index can reach a maximum of 32.2, and the smoke release can be reduced by up to 60%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a digital photo of the flame retardant material prepared in Comparative Example 1 of the present invention;

[0027] Figure 2 This is a digital photo of the flame retardant material prepared in Comparative Example 4 of the present invention;

[0028] Figure 3This is a digital photo of the flame retardant material prepared in Comparative Example 5 of the present invention;

[0029] Figure 4 This is a digital photo of the flame retardant material prepared in Comparative Example 6 of the present invention;

[0030] Figure 5 This is a digital photo of the flame retardant material prepared in Comparative Example 7 of the present invention. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0033] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0034] The invention provides a method for preparing a flame retardant material based on graphene oxide. The flame retardant material is prepared by sequentially assembling an adhesive spreading liquid, a graphene oxide solution and a phytic acid solution on a substrate by adopting a layer-by-layer self-assembly method; wherein the adhesive spreading liquid is a dendritic polyethyleneimine aqueous solution, the mass percentage of polyethyleneimine in the adhesive spreading liquid is 1-2%, and the graphene oxide solution contains 0.1-0.4% of enzymatic nanocellulose by mass percentage, 0.25-1% of graphene oxide by mass percentage and 0.05-0.1% of tannic acid by mass percentage.

[0035] Specifically, the method for preparing a flame retardant material based on graphene oxide comprises the following steps:

[0036] S1, preparing a 0.5-1.5% by mass aqueous solution of dendritic polyethyleneimine and a 0.5-1.0% by mass solution of phytic acid;

[0037] S2, soaking the substrate in the aqueous solution of branched polyethyleneimine obtained in step S1 for 1-30 minutes, taking it out and washing it to obtain a substrate assembled with the adhesive spreading solution; in this process, the positively charged branched polyethyleneimine can be used to make the surface of the substrate positively charged, thereby reducing the surface tension of the solution on the surface of the substrate during subsequent treatment, which is conducive to the subsequent assembly steps on the surface of the substrate;

[0038] S3, soaking the substrate assembled with the adhesive spreading liquid in step S2 in the pre-prepared graphene oxide solution and phytic acid solution in sequence, and then drying, to obtain a flame retardant material based on graphene oxide.

[0039] Preferably, in step S2, the types of substrates include woven fabrics, knitted fabrics, nonwovens, polyurethane foams, wood, aerogels, etc., and the types of fabric fibers include cotton, wool, silk, linen, polyester, viscose, nylon, etc.; the bath ratio of the substrate to the aqueous solution of dendritic polyethyleneimine is 1:(20-80).

[0040] Preferably, in step S3, the bath ratio of the substrate to the graphene oxide solution is 1:(50-100), and the bath ratio of the substrate to the phytic acid solution is 1:(50-100); the immersion time of the substrate in the graphene oxide solution and the phytic acid solution is 1-30 min.

[0041] Wherein, the preparation of graphene oxide solution comprises the following steps:

[0042] (1) dissolving enzymatically processed nanocellulose in water and dispersing the nanocellulose uniformly to obtain an enzymatically processed nanocellulose solution; dissolving graphene oxide in water and dispersing the nanocellulose uniformly to obtain a graphene oxide solution;

[0043] (2) Under continuous stirring, the graphene oxide solution prepared in step S1 is slowly poured into the enzymatic nanocellulose solution, and mixed evenly to obtain a mixed solution; then, tannic acid powder is added to the mixed solution, and mixed evenly to obtain a graphene oxide solution.

[0044] The preparation method of the flame retardant material based on graphene oxide of the present invention is further described below in conjunction with specific embodiments:

[0045] Example 1

[0046] This embodiment prepares a flame retardant material based on graphene oxide, and the specific preparation method includes the following steps:

[0047] S1. preparing a 1.0% by mass aqueous solution of dendritic polyethyleneimine and a 1.0% by mass solution of phytic acid;

[0048] S2, treating the polyester fabric with a sodium hydroxide solution of 2-4% by mass at 60°C for 60 minutes, soaking it in the aqueous solution of branched polyethyleneimine obtained in step S1 for 10 minutes, taking it out and washing it to obtain the polyester fabric assembled with branched polyethyleneimine; in this process, the positively charged branched polyethyleneimine can be used to make the surface of the polyester fabric positively charged, thereby reducing the surface tension of the solution on the surface of the polyester fabric during the subsequent treatment process, which is conducive to the subsequent assembly steps on the surface of the polyester fabric; wherein the bath ratio of the polyester fabric to the aqueous solution of branched polyethyleneimine is 1:50; it should be noted that the alkaline treatment of the fabric surface with sodium hydroxide solution in this step is to remove impurities on the fabric surface and expose the negatively charged -OH on the fabric surface, so as to utilize the electrostatic adsorption between it and the positively charged branched polyethyleneimine to assemble the branched polyethyleneimine on the fabric surface. In other embodiments, when the substrate surface itself contains sufficient negative charge or has adsorption capacity, the alkaline treatment step here can be omitted;

[0049] S3. Soak the polyester fabric assembled with the base layer in step S2 in the pre-prepared graphene oxide solution and phytic acid solution for 1 min, and then dry it to obtain a flame retardant material based on graphene oxide; wherein, in this step, the bath ratio of the polyester fabric to the graphene oxide solution is 1:30, and the bath ratio of the polyester fabric to the phytic acid solution is 1:50.

[0050] Wherein, the preparation of graphene oxide solution comprises the following steps:

[0051] (1) dissolving enzymatic nanocellulose in water and dispersing the nanocellulose uniformly to obtain an enzymatic nanocellulose solution with a mass percentage of 0.4%; dissolving graphene oxide in water and dispersing the nanocellulose uniformly to obtain a graphene oxide solution with a mass percentage of 1%;

[0052] (2) Under continuous stirring, the graphene oxide solution prepared in step S1 is slowly poured into the enzymatic nanocellulose solution, and mixed evenly to obtain a mixed solution; then, 0.4 g of tannic acid powder is added to the mixed solution, and mixed evenly to obtain a graphene oxide solution, wherein the mass percentage of enzymatic nanocellulose in the graphene oxide solution is 0.2%, the mass percentage of graphene oxide is 0.5%, and the mass percentage of tannic acid is 0.1%.

[0053] The present invention evaluates the performance of the material by testing the conductivity and flame retardant performance of the flame retardant material, and the flame retardant performance is evaluated by parameters such as limiting oxygen index, smoke release and flame spread rate; wherein the conductivity is obtained by testing an instrument consisting of a DC voltage-stabilized power supply (PR18-1.2A, Kenwood, Japan), a digital multimeter (8845A, Fluke, USA) equipped with a digital filter, and a small multimeter (87V, Fluke, USA), the size of the sample is 100×10mm, and during the test, two electrodes are connected to the two ends of the sample, and the knife-shaped electrode is placed on the sample, and the distance between the electrodes is 12.7mm. Current is applied to the sample through the terminal electrode, and the voltage drop between the knife electrodes is measured, and the resistance and resistivity are calculated. The conductivity is the reciprocal of the resistivity, and the test is performed on both sides of the sample, and each sample is tested at least 3 times. The limiting oxygen index test is carried out in accordance with GB / T 5454-1997, and 5 pieces of 25×6cm in size are used during the test. 2 The sample is tested. In the oxygen-nitrogen mixed gas flow, the minimum oxygen concentration required to maintain the combustion of the sample is defined as the limiting oxygen index; the horizontal flame spread test is carried out in accordance with ASTM D 4986. During the test, a 100×50mm 2 The sample is placed in a metal frame and tilted 45° in the direction of its long axis. Then a 40mm methane flame is used to ignite the short side for 6s. During the test, the burning time, combustion performance and other parameters are recorded. Each sample is tested at least 3 times. The smoke release test is carried out according to ISO 5660 standard. Each sample is cut into a 100×100mm square and the flame is heated at 50kW / m 2 The samples were placed horizontally with a radiant heat flux to study their combustion behavior, with each sample tested at least three times.

[0054] Example 2

[0055] The only difference between Example 2 and Example 1 is that the mass percentage of the phytic acid solution used in preparing the flame retardant material is 0.5%, and the other steps are basically the same as those in Example 1 and will not be repeated here.

[0056] Comparative Example 1

[0057] The only difference between Comparative Example 1 and Example 1 is that no phytic acid solution is added when preparing the flame retardant material, and the other steps are basically the same as those in Example 1, which will not be repeated here.

[0058] Comparative Examples 2 to 3

[0059] The difference between Comparative Examples 2 to 3 and Comparative Example 1 is that when preparing the graphene oxide solution, the concentrations of the enzymatic nanocellulose solution and the graphene oxide solution and the mass of the tannic acid powder are different from those in Comparative Example 1, and the other steps are basically the same as those in Comparative Example 1, which will not be repeated here. The raw material compositions for preparing the graphene oxide solution in Comparative Examples 1 to 3 are shown in Table 1.

[0060] Table 1 Raw material composition when preparing graphene oxide solution in Comparative Examples 1 to 3

[0061]

[0062] Comparative Example 4

[0063] The only difference between Comparative Example 4 and Comparative Example 1 is that when preparing the graphene oxide solution, tannic acid powder is not added, and the other steps are basically the same as those in Comparative Example 1, which will not be repeated here.

[0064] Comparative Example 5

[0065] The only difference between Comparative Example 5 and Comparative Example 1 is that when preparing the graphene oxide solution, the enzymatic nanocellulose is replaced with carboxymethyl nanocellulose, and the other steps are basically the same as those in Comparative Example 1, which will not be repeated here.

[0066] Comparative Example 6

[0067] The only difference between Comparative Example 6 and Comparative Example 1 is that when preparing the graphene oxide solution, the enzymatic nanocellulose is replaced with carboxymethyl nanocellulose, and no tannic acid powder is added. The other steps are basically the same as those in Comparative Example 1 and will not be repeated here.

[0068] Comparative Example 7

[0069] The only difference between Comparative Example 7 and Comparative Example 1 is that when preparing the graphene oxide solution, no enzymatic nanocellulose is added, and the other steps are basically the same as those in Comparative Example 1, which will not be repeated here.

[0070] The electrical conductivity and flame retardant properties of the flame retardant materials prepared in Examples 1 to 2 and Comparative Examples 1 to 7 are shown in Table 2 and Table 3, respectively. The digital photo of the flame retardant material prepared in Comparative Example 1 is shown in Figure 1 As shown, the digital photos of the flame retardant materials obtained in Comparative Examples 4 to 7 are as follows Figures 2 to 5 As shown; the test process also compared it with the original polyester fabric that had not been assembled and modified. It can be seen from Table 2 that the electrical conductivity of the flame retardant materials and the original polyester fabric prepared in Comparative Examples 4 to 7 is close to 0, and the front and back sides of the flame retardant material prepared in Example 1 have excellent electrical conductivity. This is because under the conditions of Comparative Examples 4 to 7, the graphene oxide solution cannot form a uniform coating on the surface of the polyester fabric, and the graphene oxide appears in the form of aggregation on the surface of the polyester fabric, and cannot show electrical conductivity. Combined Figures 1 to 5 As shown, Figure 1 The graphene oxide solution forms a uniform coating on the fabric surface. Figures 2 to 5 The coating on the surface of the fabric has different degrees of "peeling" and cracking. This result further verifies the above conclusion. The reasons for the above phenomenon are: in Example 1, the use of enzymatic nanocellulose to disperse graphene oxide can use enzymatic nanocellulose to disperse graphene oxide well, and obtain a graphene oxide solution with excellent dispersibility and ductility, which improves the compatibility between graphene oxide and fabric, facilitates the assembly process, and effectively improves the assembly efficiency; in addition, the addition of tannic acid can improve the aggregation tendency of graphene oxide during drying in layer-by-layer self-assembly, and avoids the self-aggregation of graphene oxide during the drying process, which affects the performance of graphene oxide in flame retardant materials. It should be noted that the front and back sides described above are only used to distinguish the two side planes of the flame retardant material, rather than limiting the flame retardant material.

[0071] The flame retardant properties of the flame retardant materials obtained in Examples 1 to 2 and Comparative Examples 1 to 3 are shown in Table 3. Combining the flame retardant properties and conductivity values ​​of the flame retardant materials obtained in Example 1 and Comparative Example 1 in Table 3 and Table 2, it can be seen that the presence of the phytic acid solution coating in the flame retardant material has little effect on the conductivity, but can improve the flame retardant properties of the flame retardant material. This result also further illustrates that the introduction of the phytic acid solution coating will not affect the uniformity of the graphene oxide solution coating. As can be seen from Table 3, the flame retardant material prepared by the preparation method of the flame retardant material based on graphene oxide proposed in the present invention has excellent flame retardant and smoke suppression functions and anti-melting droplet effects. The flame retardant material can reach a limiting oxygen index (LOI) of 30.6 at a minimum weight gain of 8.9%, and the LOI can reach up to 32.2, and the smoke release can be reduced by up to 60%. The results show that the flame retardant material prepared by the preparation method proposed in the present invention has excellent flame retardant properties and can well slow down the spread of flames.

[0072] Table 2 Electrical conductivity of flame retardant materials obtained in Examples 1 to 2 and Comparative Examples 1 to 7

[0073]

[0074]

[0075] Table 3 Flame retardant properties of flame retardant materials obtained in Examples 1 to 2 and Comparative Examples 1 to 3

[0076]

[0077] In summary, the preparation method of the flame retardant material based on graphene oxide proposed in the present invention is to obtain a graphene oxide solution with good ductility by first dispersing graphene oxide using enzymatic nanocellulose and then adding tannic acid to change the aggregation tendency of graphene oxide, and then assemble the adhesive spreading liquid, graphene oxide solution and phytic acid solution on the substrate in sequence by using the layer-by-layer self-assembly method. In the above process, by regulating the ratio of the adhesive spreading liquid, graphene oxide solution and phytic acid solution during the layer-by-layer self-assembly process, it is ensured that each layer is evenly distributed on the surface of the substrate and the layers are firmly bonded. In the above manner, a flame retardant material based on graphene oxide with uniform coating and excellent flame retardant properties is obtained.

[0078] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a flame retardant material based on graphene oxide, characterized in that: The flame retardant material is prepared by assembling an adhesive spreading liquid, a graphene oxide solution and a phytic acid solution on a substrate in sequence by adopting a layer-by-layer self-assembly method; the adhesive spreading liquid is a dendritic polyethyleneimine aqueous solution, and the graphene oxide solution contains enzymatic nanocellulose, graphene oxide and tannic acid; The steps include: S1, preparing the dendritic polyethyleneimine aqueous solution, the phytic acid solution and the graphene oxide solution; the mass percentage of the dendritic polyethyleneimine in the dendritic polyethyleneimine aqueous solution is 1-2%, and the mass percentage of the phytic acid solution is 0.5-1.0%; S2, soaking the substrate in the aqueous solution of dendritic polyethyleneimine obtained in step S1 for 1-30 minutes, taking it out and washing it to obtain a substrate assembled with the adhesive spreading solution; S3, soaking the substrate assembled with the adhesive spreading liquid in step S2 in the pre-prepared graphene oxide solution and the phytic acid solution, and then drying, thereby obtaining a flame retardant material based on graphene oxide; In step S1, the preparation of the graphene oxide solution comprises the following steps: (1) dissolving enzymatically processed nanocellulose in water and dispersing the nanocellulose uniformly to obtain an enzymatically processed nanocellulose solution; dissolving graphene oxide in water and dispersing the nanocellulose uniformly to obtain a graphene oxide solution; (2) under continuous stirring, slowly pouring the graphene oxide solution prepared in step S1 into the enzymatic nanocellulose solution, and mixing them evenly to obtain a mixed solution; then, adding tannic acid powder to the mixed solution, and mixing them evenly to obtain the graphene oxide solution; The mass percentage of the enzymatic nanocellulose in the graphene oxide solution is 0.1-0.4%, the mass percentage of the graphene oxide is 0.25-1%, and the mass percentage of the tannic acid is 0.05-0.1%.

2. The method for preparing a flame retardant material based on graphene oxide according to claim 1, characterized in that: In step S3, the bath ratio of the substrate to the graphene oxide solution is 1:(50-100), and the bath ratio of the substrate to the phytic acid solution is 1:(50-100).

3. The method for preparing a flame retardant material based on graphene oxide according to claim 1, characterized in that: In step S2, the bath ratio of the substrate to the aqueous solution of dendritic polyethyleneimine is 1:(20-80).

4. The method for preparing a flame retardant material based on graphene oxide according to claim 1, characterized in that: In step S2, the substrate is further subjected to alkali treatment before being immersed in the aqueous solution of dendritic polyethyleneimine. The alkali treatment is performed using a sodium hydroxide solution with a mass percentage of 2-4%. The temperature of the alkali treatment is 60°C and the time is 60 minutes.

5. The method for preparing a flame retardant material based on graphene oxide according to claim 1, characterized in that: In step S3, the substrate is immersed in the graphene oxide solution and the phytic acid solution for 1-30 minutes.

6. The method for preparing a flame retardant material based on graphene oxide according to claim 1, characterized in that: The types of the substrate include woven fabrics, knitted fabrics, nonwoven fabrics, polyurethane foam, wood, and aerogels, and the types of fabric fibers include cotton, wool, silk, linen, polyester, viscose, and nylon.