A biochar based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration and its preparation method and application

Through the pyrolysis treatment of canna hydrothermal carbon, biochar with high cadmium adsorption capacity was prepared, which solved the harmless problem of solid waste after hydrothermal carbon treatment, and improved the cadmium adsorption efficiency, achieving efficient treatment of polluted water .

CN116351390BActive Publication Date: 2024-11-08TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111569260.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-21
Publication Date
2024-11-08
Estimated Expiration
2041-12-21

AI Technical Summary

Technical Problem

In the prior art, when treating cadmium-containing contaminated water, the adsorbed hydrothermal carbon becomes solid waste due to its rich metals, which lacks research on harmless treatment and resource utilization, and its cadmium adsorption capacity is limited, making it difficult to effectively remove pollution. .

Method used

Hydrothermal carbon is prepared by hydrothermal carbonizing canna powder, and then cadmium adsorption is performed and pyrolytic treatment is performed under a nitrogen atmosphere to prepare biochar pyrolytic hydrothermal carbon to improve quality and regenerate, thereby improving its cadmium adsorption ability. The method includes the preparation of canna powder, hydrothermal carbonization, cadmium adsorption and pyrolysis treatment, and the resulting biochar has a higher cadmium adsorption capacity.

Benefits of technology

It has achieved harmless treatment and quality improvement and reuse of canna hydrothermal carbon, significantly improved the cadmium adsorption capacity, efficiently removed heavy metal cadmium, reduced the risk of secondary pollution, and was easy to operate and green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for preparing biochar based on pyrolysis and regeneration of hydrothermal carbon for cadmium adsorption, the method comprising: preparing canna powder; mixing the canna powder with deionized water, and then hydrothermal carbonizing to obtain hydrothermal carbon; placing the hydrothermal carbon in a heavy metal cadmium solution for adsorption, collecting the hydrothermal carbon after adsorbing the heavy metal cadmium, and obtaining hydrothermal carbon adsorbing cadmium; placing the hydrothermal carbon adsorbing cadmium in a nitrogen atmosphere, pyrolyzing at 700-900°C, removing the cadmium adsorbed in the hydrothermal carbon adsorbing cadmium, and collecting the pyrolyzed carbon after pyrolysis, and obtaining biochar based on pyrolysis and regeneration of hydrothermal carbon adsorbing cadmium. The invention uses the water body remediation plant canna to prepare hydrothermal carbon for heavy metal cadmium adsorption, and then removes the cadmium in the hydrothermal carbon adsorbing cadmium through heat treatment, so that the obtained regenerated biochar has a higher cadmium adsorption capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid waste resource utilization and environmental protection, and in particular to a biochar based on cadmium adsorption hydrothermal charcoal pyrolysis upgrading and regeneration, and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of non-ferrous metal smelting, electroplating and other industries, more and more water resources have been polluted by heavy metal ions. Among the many heavy metals, cadmium is not only a recognized highly toxic substance, but also the first category of harmful substances strictly controlled in the pollutant emission standards. Cadmium in the environment will enter the human body through the digestive tract, respiratory tract and skin, and then form cadmium sulfide protein in the body, reach the whole body through the blood circulation, and selectively accumulate in the kidneys and liver, endangering human health. Therefore, cadmium pollution treatment has attracted much attention.

[0003] At present, the technologies for removing heavy metal cadmium from sewage include adsorption, chemical precipitation, membrane separation, reverse osmosis and ion exchange. Among them, adsorption technology is widely used to treat wastewater containing heavy metal pollution due to its advantages such as simple operation and low investment cost. Hydrothermal carbon has been often used as one of the typical adsorbents for removing heavy metal cadmium in recent years because of its more oxygen-containing functional groups and considerable specific surface area. Canna hydrothermal carbon, as a kind of hydrothermal carbon, has attracted much attention as a very promising adsorption material due to its wide source of raw materials and low cost. After Canna hydrothermal carbon is used to adsorb heavy metal cadmium, it will become solid waste due to its rich heavy metal content. If it is not handled properly, it will cause secondary pollution, but there is almost no research on its harmless treatment and resource utilization. Summary of the invention

[0004] The present invention provides a biochar based on pyrolysis and regeneration of hydrothermal carbon with cadmium adsorption, and a preparation method and application thereof. The biochar based on pyrolysis and regeneration of hydrothermal carbon with cadmium adsorption has a higher cadmium adsorption capacity than the hydrothermal carbon before regeneration.

[0005] The specific technical solutions are as follows:

[0006] A method for preparing biochar based on cadmium adsorption hydrothermal carbon pyrolysis and quality improvement regeneration, comprising the following steps:

[0007] (1) preparing canna powder;

[0008] (2) mixing the canna powder with deionized water and then performing hydrothermal carbonization to obtain hydrothermal charcoal;

[0009] (3) placing the hydrothermal carbon in a heavy metal cadmium solution for adsorption, collecting the hydrothermal carbon after the heavy metal cadmium is adsorbed, and obtaining the hydrothermal carbon adsorbed with cadmium;

[0010] (4) placing the hydrothermal carbon adsorbing cadmium in a nitrogen atmosphere and pyrolyzing it at 700-900°C to remove the cadmium adsorbed in the hydrothermal carbon adsorbing cadmium, and collecting the pyrolyzed carbon after pyrolysis to obtain biochar based on the pyrolysis and regeneration of the cadmium adsorbed hydrothermal carbon.

[0011] Hydrothermal carbonization of Canna refers to the use of Canna biomass in the subcritical state or supercritical state of water to decompose into hydrothermal charcoal under oxygen-free and high-pressure conditions. Pyrolysis refers to the thermal decomposition process of substances under oxygen-free and high-temperature conditions. Hydrothermal charcoal and pyrolytic charcoal are the products of hydrothermal carbonization and pyrolysis, respectively. The yield of hydrothermal charcoal and pyrolytic charcoal and their adsorption capacity for heavy metal cadmium have strict requirements on operation and are better under specific conditions.

[0012] Preferably, in step (1), the preparation method of the canna powder is: take the harvested canna plants, remove impurities, wash and air-dry, and then dry, crush and sieve in sequence to obtain the canna powder. The appropriate temperature and time during the canna drying process are the factors that determine the biomass crushing effect and the hydrothermal reaction effect; therefore, preferably, the drying temperature is 65-105°C and the time is 23-24h.

[0013] Preferably, the moisture content of the canna after air-drying in step (1) is less than 20%.

[0014] The particle size of the crushed canna is related to the degree of hydrothermal carbonization. If the particle size is too large, the hydrothermal carbonization of the canna may be incomplete. Preferably, the crushed canna in step (1) is passed through a 40-mesh sieve.

[0015] The mass ratio of canna powder to deionized water in step (2) has a certain relationship with the hydrothermal carbon yield and the adsorption performance of the hydrothermal carbon to heavy metal cadmium. Preferably, in step (2), the mixing ratio of the canna powder to deionized water is 1:8 to 1:12.

[0016] Preferably, in step (2), the heating rate of the hydrothermal carbonization is 5-20°C / min, and the temperature is raised to 195-205°C and then kept warm for 1.5-2.5h; after the hydrothermal carbonization, the mixed solution is cooled to room temperature, the material is taken out and filtered, and the solid product after filtration is dried and crushed to obtain hydrothermal charcoal.

[0017] After hydrothermal carbonization, in order to increase the contact area between the hydrothermal carbon and the cadmium solution to be adsorbed and thus improve its adsorption performance, preferably, the pulverized product in step (2) is sieved through a 40-mesh sieve.

[0018] Preferably, in step (3), the concentration of cadmium ions in the heavy metal cadmium solution is 195-205 mg / L; the mass ratio of the hydrothermal carbon to the heavy metal cadmium solution is 1:995-1:1005; the hydrothermal carbon after adsorbing the heavy metal cadmium is collected, dried and crushed to obtain hydrothermal carbon adsorbed with cadmium; the drying temperature and time of the hydrothermal carbon after adsorbing cadmium are important factors affecting the preparation of pyrolytic carbon in the next step, and preferably, the drying temperature is 65-105°C and the time is 23-24 h; and the crushed carbon is sieved through a 40-mesh sieve.

[0019] Preferably, in step (4), the flow rate of the nitrogen is 0.18 to 0.22 L / min, the heating rate of the pyrolysis is 5 to 10°C / min, and the temperature is raised to 700 to 900°C and then maintained for 1.5 to 2.5 hours.

[0020] The present invention also provides biochar based on cadmium adsorption hydrothermal carbon pyrolysis and quality upgrading and regeneration, which is prepared by the preparation method as described above, wherein the pH of the biochar is 11.98-12.24, the ash content is 20.3%-21.5%, and the adsorption amount of heavy metal cadmium is 29.12-35.83 mg / g.

[0021] The present invention also provides the use of the biochar based on cadmium adsorption hydrothermal carbon pyrolysis and quality upgrading and regeneration in treating water bodies contaminated by heavy metal cadmium.

[0022] Preferably, the application includes: based on the mass percentage of heavy metal cadmium in the cadmium solution, the amount of biochar added is 0.09-0.1% of the heavy metal cadmium solution.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses the water body remediation plant Canna indica to prepare hydrothermal charcoal for heavy metal cadmium adsorption, and then removes the heavy metal cadmium in the hydrothermal charcoal that has adsorbed cadmium through heat treatment, so that the prepared biochar has a higher cadmium adsorption capacity.

[0025] (2) The present invention uses canna as the raw material for preparing hydrothermal charcoal. The method is easy to operate and is green and environmentally friendly. It not only realizes the harmlessness and reuse of plant waste, but also can reprocess the hydrothermal charcoal adsorbed with cadmium, which is a solid waste turned into harmless due to the adsorption of cadmium, and realizes quality improvement and reuse. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments. The following are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto.

[0027] In the following examples and comparative examples, the processing steps and calculation methods involved in cadmium adsorption are as follows:

[0028] Weigh 30 mg of the prepared hydrochar or biochar based on cadmium adsorption hydrochar pyrolysis and regeneration into a 50 mL glass bottle, then add 30 mL of 200 mg / L cadmium solution and oscillate the mixture at 25 ° C for 24 h, wherein the initial pH of the cadmium solution is 5 and 0.01 mol / L NaNO3 is used as the background electrolyte. After oscillation for 24 h, the mixture is filtered with a 0.45 μm filter membrane and the filtered solution is collected, and then the content of heavy metal cadmium in the solution before and after 24 h of oscillation is determined by ICP-OES, and the adsorption amount of cadmium by hydrochar or biochar based on cadmium adsorption hydrochar pyrolysis and regeneration is calculated, and the calculation formula is: adsorption amount = (concentration of prepared cadmium solution - residual cadmium concentration in the solution after 24 h) * volume of cadmium solution during adsorption / mass of hydrochar or biochar based on cadmium adsorption hydrochar pyrolysis and regeneration.

[0029] In the following examples, the determination steps and calculation methods of the physical and chemical properties of biochar based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration are as follows:

[0030] The yield of all prepared biochars based on pyrolysis and regeneration of cadmium-adsorbing hydrothermal carbon was calculated by the formula: Yield = (weight of biochar prepared after pyrolysis based on pyrolysis and regeneration of cadmium-adsorbing hydrothermal carbon / weight of hydrothermal carbon that adsorbed cadmium before pyrolysis).

[0031] Weigh 0.2 g of the biochar prepared by pyrolysis and regeneration of cadmium-adsorbing hydrothermal carbon, mix it with 4 ml of deionized water and shake it for 24 hours, then let it stand and measure the pH of the supernatant, which is the pH of the sample.

[0032] Weigh 0.3 g of the prepared biochar based on cadmium adsorption hydrothermal charcoal pyrolysis and regeneration and put it into a muffle furnace, then heat the muffle furnace to 750°C, and burn the hydrothermal charcoal or the biochar based on cadmium adsorption hydrothermal charcoal pyrolysis and regeneration at this temperature for 6 hours. After the reaction is completed, the weight of the remaining sample is measured, and the ash content is calculated as follows: ash content = (weight of the sample after the reaction is completed / 0.3*100%).

[0033] The carbon and nitrogen contents of the biochar samples prepared by pyrolysis and regeneration of biochar based on cadmium adsorption hydrothermal carbon were determined using an elemental analyzer.

[0034] In the following embodiments, the steps and calculation methods for determining the cadmium content and cadmium removal rate in biochar based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration are as follows:

[0035] Weigh 0.2g of the prepared hydrothermal charcoal after cadmium adsorption or the biochar based on the pyrolysis and regeneration of the cadmium-adsorbed hydrothermal charcoal, digest it with a digester and use ICP-OES to measure the cadmium content in different samples, so as to obtain the cadmium content in the hydrothermal charcoal adsorbing cadmium and the biochar based on the pyrolysis and regeneration of the cadmium-adsorbed hydrothermal charcoal, and use the formula: The removal rate of heavy metal cadmium in hydrothermal charcoal relative to the adsorption of heavy metal cadmium = (1-the cadmium content of biochar based on the pyrolysis and regeneration of cadmium-adsorbed hydrothermal charcoal * the yield of biochar based on the pyrolysis and regeneration of cadmium-adsorbed hydrothermal charcoal / the cadmium content in the hydrothermal charcoal adsorbing cadmium) * 100%.

[0036] Example 1

[0037] 1. Preparation of biochar

[0038] The specific steps are as follows:

[0039] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0040] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a heating rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal.

[0041] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0042] (4) The hydrothermal carbon adsorbed with cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is raised to 700°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar prepared at 700°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon.

[0043] 2. Treatment of cadmium-containing wastewater

[0044] Take 30 mg of biochar prepared at 700°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in the cadmium solution again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 700°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0045] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0046] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 700°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 700°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0047] In this embodiment, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 700°C. As shown in Table 1, the yield was 47.6%, the pH was 12.20, the ash content was 20.3%, the carbon content was 69.11%, and the nitrogen content was 2.21%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 10.71 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 99.92%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by the biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared at 700°C in this embodiment was 30.87 mg / g.

[0048] Example 2

[0049] 1. Preparation of biochar

[0050] The specific steps are as follows:

[0051] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0052] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200°C at a rate of 5 to 20°C / min and kept at that temperature for 2 hours for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal.

[0053] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0054] (4) The hydrothermal carbon adsorbed with cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is increased to 800°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar prepared at 800°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon.

[0055] 2. Treatment of cadmium-containing wastewater

[0056] Take 30 mg of biochar prepared at 800°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in cadmium-containing wastewater again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 800°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0057] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0058] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 800°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 800°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0059] In this embodiment, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 800°C. As shown in Table 1, the yield was 46.4%, the pH was 12.24, the ash content was 21.5%, the carbon content was 70.43%, and the nitrogen content was 1.65%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 9.80 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 99.93%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared by this embodiment at 800°C was 35.73 mg / g.

[0060] Example 3

[0061] 1. Preparation of biochar

[0062] The specific steps are as follows:

[0063] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0064] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixture was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal;

[0065] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0066] (4) The hydrothermal carbon adsorbed with cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is raised to 900°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar prepared at 900°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon.

[0067] 2. Treatment of cadmium-containing wastewater

[0068] Take 30 mg of biochar prepared at 900°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in cadmium-containing wastewater again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 900°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0069] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0070] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 900°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 900°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0071] In this embodiment, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 900°C. As shown in Table 1, the yield was 45.8%, the pH was 11.98, the ash content was 21.17%, the carbon content was 70.66%, and the nitrogen content was 1.31%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 4.30 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 99.97%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared by this embodiment at 900°C was 29.12 mg / g.

[0072] Comparative Example 1

[0073] 1. Preparation of hydrothermal charcoal

[0074] The specific steps are as follows:

[0075] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0076] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a rate of 5 to 20° C. and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal.

[0077] 2. Treatment of cadmium-containing wastewater

[0078] Take 30 mg of the prepared canna hydrothermal charcoal, mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and oscillate it for 24 hours to adsorb cadmium in the cadmium-containing wastewater again; as shown in Table 3, the adsorption amount of heavy metal cadmium in the cadmium-containing solution by the hydrothermal charcoal prepared in this comparative example is 5.5 mg / g.

[0079] Comparative Example 2

[0080] 1. Preparation of biochar

[0081] The specific steps are as follows:

[0082] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0083] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a heating rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal.

[0084] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0085] (4) The hydrothermal carbon adsorbing cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is increased to 300°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar regenerated by pyrolysis of cadmium-adsorbed hydrothermal carbon at 300°C.

[0086] 2. Treatment of cadmium-containing wastewater

[0087] Take 30 mg of biochar prepared at 300°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in cadmium-containing wastewater again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 300°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0088] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0089] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 300°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 300°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0090] In this comparative example, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 300°C. As shown in Table 1, the yield was 78.1%, the pH was 6.53, the ash content was 13.18%, the carbon content was 61.52%, and the nitrogen content was 2.36%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 7875 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 8.75%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared at 300°C by this comparative example was 0.72 mg / g.

[0091] Comparative Example 3

[0092] 1. Preparation of biochar

[0093] The specific steps are as follows:

[0094] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0095] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal carbon.

[0096] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0097] (4) The hydrothermal carbon adsorbing cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is increased to 400°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar regenerated by pyrolysis of cadmium-adsorbed hydrothermal carbon at 400°C.

[0098] 2. Treatment of cadmium-containing wastewater

[0099] Take 30 mg of biochar prepared at 400°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and oscillate for 24 hours to adsorb cadmium in cadmium-containing wastewater again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 400°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0100] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0101] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 400°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 400°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0102] In this comparative example, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 400°C. As shown in Table 1, its yield was 58.5%, pH was 8.01, ash content was 16.6%, carbon content was 62.66%, and nitrogen content was 2.66%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 8146.7 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon relative to the adsorption of heavy metal cadmium was 29.28%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared at 400°C by this comparative example was 2.02 mg / g.

[0103] Comparative Example 4

[0104] 1. Preparation of biochar

[0105] The specific steps are as follows:

[0106] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0107] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixture was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal;

[0108] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0109] (4) The hydrothermal carbon adsorbed with cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is raised to 500°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar prepared at 500°C based on the pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon.

[0110] 2. Treatment of cadmium-containing wastewater

[0111] Take 30 mg of biochar prepared at 500°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in cadmium-containing wastewater again; and use the canna hydrothermal carbon prepared in step (2) as a control to determine the cadmium adsorption content of canna hydrothermal carbon and biochar prepared at 500°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and the results are shown in Table 3.

[0112] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0113] The above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the yield of the biochar prepared at 500°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar, as shown in Table 1; the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon were used to determine the cadmium content in the biochar prepared at 500°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium, and the results are shown in Table 2.

[0114] In this comparative example, biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon was prepared at 500°C. As shown in Table 1, the yield was 53.5%, the pH was 8.94, the ash content was 18.1%, the carbon content was 67.17%, and the nitrogen content was 2.86%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 3529.70 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 72.00%. As shown in Table 3, the biochar based on pyrolysis and regeneration of cadmium adsorption hydrothermal carbon prepared by this comparative example at 500°C had an adsorption capacity of 2.52 mg / g of cadmium in the cadmium-containing solution.

[0115] Comparative Example 5

[0116] 1. Preparation of biochar

[0117] The specific steps are as follows:

[0118] (1) harvesting canna plants, removing impurities, washing, air-drying, drying at 65-105° C., crushing, and sieving to obtain canna powder;

[0119] (2) 10 g of canna biomass powder was mixed with deionized water in a ratio of 1:10 and placed in a hydrothermal reaction device. After nitrogen was introduced to remove oxygen, the reaction device was turned on and the temperature was raised to 200° C. at a heating rate of 5 to 20° C. / min and kept at that temperature for 2 h for hydrothermal carbonization. After hydrothermal carbonization, the mixed solution was cooled to room temperature, the material was taken out and filtered, and the solid product after filtration was dried and crushed to obtain canna hydrothermal charcoal.

[0120] (3) taking the hydrothermal carbon of step (2) and a heavy metal cadmium solution having a cadmium ion concentration of 200 mg / L, mixing and oscillating at a mass ratio of 1:1000 for 24 hours, filtering and collecting the hydrothermal carbon adsorbing heavy metal cadmium after the oscillation, drying at 65-105° C. for 23-24 hours, and crushing through a 40-mesh sieve to obtain hydrothermal carbon adsorbing cadmium;

[0121] (4) The hydrothermal carbon adsorbed with cadmium in step (3) is placed in a tubular furnace, and nitrogen is introduced at a nitrogen flow rate of 0.2 L / min to isolate the oxygen in the tubular furnace, while the reaction pressure is maintained at 0.01 MPa, the heating rate is set to 5°C / min, the temperature is raised to 600°C, and then kept warm for 2 hours, and the pyrolytic carbon after pyrolysis is collected to obtain biochar prepared at 600°C based on the pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon.

[0122] 2. Treatment of cadmium-containing wastewater

[0123] Take 30 mg of biochar prepared at 600°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, and mix it with a cadmium solution with a concentration of 200 mg / L at a mass ratio of 1:1000 and shake it for 24 hours to adsorb cadmium in cadmium-containing wastewater again; using the canna hydrothermal carbon prepared in step (2) as a control, the cadmium adsorption content of the canna hydrothermal carbon and the biochar prepared at 600°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration was determined, and the results are shown in Table 3.

[0124] 3. Determination of the physical and chemical properties of biochar, cadmium content, and cadmium removal rate

[0125] Using the above-mentioned determination steps and calculation methods for the physical and chemical properties of biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, the yield of the above-mentioned biochar prepared at 600°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, as well as the pH value, ash content, carbon content and nitrogen content of the biochar were determined, and the results are shown in Table 1; using the above-mentioned determination steps and calculation methods for the cadmium content and cadmium removal rate in biochar based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon, the cadmium content in the biochar prepared at 600°C based on pyrolysis and regeneration of cadmium-adsorbed hydrothermal carbon and the removal rate of heavy metal cadmium in the hydrothermal carbon that relatively adsorbed heavy metal cadmium were determined, and the results are shown in Table 2.

[0126] In this comparative example, biochar based on pyrolysis and regeneration of cadmium adsorbed hydrothermal carbon was prepared at 600°C. As shown in Table 1, its yield was 50.2%, pH was 9.79, ash content was 19.0%, carbon content was 68.39%, and nitrogen content was 2.63%. As shown in Table 2, the heavy metal cadmium contained in the biochar was 133.75 mg / kg, and the removal rate of heavy metal cadmium in the hydrothermal carbon adsorbed heavy metal cadmium was 99.00%. As shown in Table 3, the adsorption of cadmium in the cadmium-containing solution by the biochar based on pyrolysis and regeneration of cadmium adsorbed hydrothermal carbon prepared by this comparative example at 600°C was 8.52 mg / g.

[0127] Table 1 Physical and chemical properties of the biochar prepared at 300-900 °C based on cadmium adsorption hydrothermal char pyrolysis and regeneration

[0128]

[0129] Table 2 Cadmium content in the biochar prepared at 300-900°C based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration and the removal rate of heavy metal cadmium in the hydrothermal carbon with heavy metal cadmium adsorbed

[0130]

[0131] Table 3 The adsorption of cadmium by the above hydrothermal carbon and the biochar prepared by pyrolysis and regeneration of hydrothermal carbon based on cadmium adsorption at 300-900°C

[0132]

Claims

1. A method for preparing biochar based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration, characterized in that: The following steps are involved: (1) preparing canna powder; (2) mixing the canna powder with deionized water and then performing hydrothermal carbonization to obtain hydrothermal charcoal; (3) placing the hydrothermal carbon in a heavy metal cadmium solution for adsorption, collecting the hydrothermal carbon after the heavy metal cadmium is adsorbed, and obtaining the hydrothermal carbon adsorbed with cadmium; In the heavy metal cadmium solution, the concentration of cadmium ions is 195-205 mg / L; the mass ratio of the hydrothermal carbon to the heavy metal cadmium solution is 1:995-1:1005; The hydrothermal carbon after adsorbing heavy metal cadmium is collected, dried and crushed to obtain hydrothermal carbon adsorbing cadmium; the drying temperature is 65-105° C.; (4) placing the hydrothermal carbon adsorbed with cadmium in a nitrogen atmosphere, pyrolyzing it at 700-900° C., removing the cadmium adsorbed in the hydrothermal carbon adsorbed with cadmium, and collecting the pyrolyzed carbon after pyrolysis to obtain biochar based on pyrolysis and regeneration of the cadmium adsorbed hydrothermal carbon; The flow rate of the nitrogen is 0.18-0.22 L / min, the heating rate of the pyrolysis is 5-10° C. / min, and the temperature is heated to 700-900° C. and then kept warm for 1.5-2.5 hours.

2. The preparation method according to claim 1, characterized in that In step (1), the preparation method of the canna powder is as follows: harvested canna plants are taken, impurities are removed, washed and air-dried, and then dried, crushed and sieved in sequence to obtain canna powder; the drying temperature is 65-105°C.

3. The preparation method according to claim 1, characterized in that: In step (2), the mixing ratio of the canna powder and deionized water is 1:8 to 1:

12.

4. The preparation method according to claim 1, characterized in that: In step (2), the heating rate of the hydrothermal carbonization is 5 to 20°C / min, and the temperature is raised to 195 to 205°C and then kept warm for 1.5 to 2.5 hours; After hydrothermal carbonization, the mixed solution is cooled to room temperature, the material is taken out and filtered, and the solid product after filtration is dried and crushed to obtain hydrothermal carbon.

5. The biochar prepared by the preparation method according to any one of claims 1 to 4, characterized in that: The pH value of the biochar is 11.98-12.24, the ash content is 20.3%-21.5%, and the adsorption capacity of heavy metal cadmium is 29.12-35.83 mg / g.

6. The use of biochar based on cadmium adsorption hydrothermal carbon pyrolysis and regeneration as claimed in claim 5 in treating heavy metal cadmium contaminated water.

7. The use according to claim 6, characterized in that include: Calculated by the mass percentage of heavy metal cadmium in the cadmium solution, the added amount of the biochar is 0.09-0.1% of the heavy metal cadmium solution.