A catalyst for synthesizing vinyl sulfate and a method for preparing vinyl sulfate

By using RuO2/CeZrOx supported catalysts and high-purity oxygen in vinyl sulfate synthesis, the problems of low yields and environmental pollution in the prior art are solved, and efficient and environmentally friendly vinyl sulfate production is achieved, reducing production costs.

CN116351413BActive Publication Date: 2024-11-08WUXI WEIFU ENVIRONMENT PROTECTION CATALYST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310162876.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-11-08
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The existing vinyl sulfate synthesis technology has problems such as low yield, high environmental hazards, high equipment investment and precious metal losses, especially the environmental pollution and cost increase caused by the use of sodium hypochlorite and ruthenium trichloride.

Method used

Using RuO2/CeZrOx-supported catalyst, the oxidation performance and recycling times of the catalyst are improved by loading ruthenium on CeZrOx and presenting it in solid form, combining high-purity oxygen or ozone as an oxidant, and reducing the amount of precious metals used.

Benefits of technology

A high yield of vinyl sulfate (up to 94.2%) and an environmentally friendly production process have been achieved, reducing production costs and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a catalyst for synthesizing vinyl sulfate and a method for preparing vinyl sulfate. The catalyst for synthesizing vinyl sulfate of the present invention is a supported catalyst, the supported catalyst is RuO2 / CeZrOx, and the mass content of ruthenium in the catalyst is 0.1% to 10%; the catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the catalytic synthesis of vinyl sulfate. The RuO2 / CeZrOx catalyst used in the present invention exists in solid form during the catalytic synthesis of vinyl sulfate and can be recycled. After the catalyst is recycled 10 times, the yield of vinyl sulfate is higher than 90%. The supported ruthenium catalyst of the present invention has high catalytic activity and good stability. The synthetic process for catalytic synthesis of vinyl sulfate is green and environmentally friendly, with high yield, and can reduce the amount of precious metal ruthenium, thereby reducing production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vinyl sulfate synthesis, and particularly relates to a catalyst for vinyl sulfate synthesis and a method for preparing vinyl sulfate. Background Art

[0002] Vinyl sulfate is an electrolyte additive for lithium-ion batteries. Due to its excellent low-temperature performance, it is used to make low-temperature resistant lithium-ion batteries. Currently, there are several main methods for synthesizing vinyl sulfate:

[0003] 1. The reaction of dibromoethane and silver sulfate, but this method has a low yield and excessive dibromoethane will cause great environmental damage.

[0004] 2. The reaction of ethylene oxide and sulfur trioxide has a high yield. However, since strongly acidic sulfur trioxide gas is used, the equipment has extremely high corrosion resistance requirements. It is not very economical for small batches of fine chemicals. In addition, cuprous oxide is used as a catalyst in the process and can only be used once, which further increases the cost.

[0005] 3. Reaction of ethylene glycol and sulfuryl chloride: This method has cheap raw materials and high product yield, but sulfuryl chloride is a highly corrosive acid and has very high toxicity. The equipment is extremely corrosive and requires high equipment investment. It also produces a large amount of highly corrosive hydrogen chloride gas, which is harmful to the environment.

[0006] 4. Ethylene sulfite oxidation method: ruthenium trichloride is used as a catalyst, sodium hypochlorite is used as an oxidant, and water and ethylene dichloride are used as solvents. Ethylene sulfite is oxidized to vinyl sulfate. However, this process has several problems: (1) a large amount of sodium hypochlorite wastewater. This process requires a large amount of sodium hypochlorite, which causes a large amount of sodium hypochlorite to be discharged into the water body, causing great environmental damage; (2) a large amount of ruthenium trichloride catalyst is lost. Ruthenium trichloride is in the form of a solution in the catalytic system. After the reaction is completed, the ruthenium trichloride cannot be recovered and can only be calculated as a loss, resulting in a large amount of precious metal loss and environmental damage. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a catalyst for synthesizing vinyl sulfate and a method for preparing vinyl sulfate. The RuO2 / CeZrOx catalyst used in the present invention exists in a solid form during the catalytic synthesis of vinyl sulfate and can be recycled. After the catalyst is recycled 10 times, when catalytically synthesizing vinyl sulfate, the yield of vinyl sulfate is still higher than 90%.

[0008] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:

[0009] In a first aspect, an embodiment of the present invention provides a catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, wherein the supported catalyst is RuO2 / CeZrOx, and the mass content of ruthenium in the catalyst is 0.1% to 10%;

[0010] The catalyst is used for catalytic synthesis of vinyl sulfate, and in the process of catalytic synthesis of vinyl sulfate, the catalyst exists in a solid form.

[0011] Furthermore, the preparation of the RuO2 / CeZrOx catalyst comprises the following steps:

[0012] (1) adding ruthenium trichloride solid to 20-60 g of deionized water, stirring to dissolve, then adding alkaline solution, adjusting the pH value of the solution to 10-14, and continuing to stir to obtain a ruthenium hydroxide alkaline solution;

[0013] (2) adding the above ruthenium hydroxide alkaline solution dropwise to the cerium-zirconium composite oxide powder, continuing stirring for 1 hour, standing overnight, filtering and washing to remove impurity ions, and obtaining Ru(OH)3 / CeZrOx slurry;

[0014] (3) The obtained Ru(OH)3 / CeZrOx slurry is dried at 50-150°C for 1-5 h, and calcined at 300-500°C. Air containing 1-15% water vapor is first introduced for 1-5 h, and then air is introduced for 1-2 h. After the calcination, the slurry is naturally cooled to room temperature to obtain a RuO2 / CeZrOx catalyst.

[0015] Furthermore, the solute in the alkaline solution in step (1) includes one or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.

[0016] Furthermore, the mass content of cerium oxide in the cerium-zirconium composite oxide in step (2) is 0.1 to 90%.

[0017] In a second aspect, an embodiment of the present invention provides a method for preparing vinyl sulfate, comprising the following steps:

[0018] 1g of RuO2 / CeZrOx catalyst, 10-100g of vinyl sulfite, 1-1000g of ethylene dichloride and 1-500g of water are added into a reaction kettle, and an oxidant at 0.1-6MPa is introduced. The mixture is reacted at 10-80°C for 5h, filtered, cleaned and impurities removed to obtain vinyl sulfate.

[0019] Furthermore, the oxidant is high-purity oxygen or O3.

[0020] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0021] In order to overcome the deficiencies of the prior art, the present invention has made the following improvements: (1) the noble metal ruthenium is loaded onto CeZrOx to prepare a loaded catalyst; (2) the oxidant is changed from sodium hypochlorite to high-pressure, high-purity oxygen or ozone. However, since the oxidizing performance of high-pressure oxygen or ozone is relatively poor, in order to further improve the oxidizing performance of the catalyst, a cerium-zirconium composite oxide material is selected as the catalyst carrier. The active oxygen on the surface of the cerium-zirconium composite oxide material can be quickly transferred to the sulfite, further enhancing the oxidizing performance of the catalyst; (3) the RuO2 / CeZrOx catalyst exists in a solid form during the catalytic synthesis of vinyl sulfate and can be recycled. After the catalyst is recycled 10 times, the yield of vinyl sulfate is as high as 94.2%. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0023] Example 1

[0024] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0025] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0026] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0027] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the solution pH to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0028] (2) The above ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and then filtered and washed to remove impurity ions to obtain Ru(OH)3 / CeZrOx slurry.

[0029] (3) The obtained Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly introduced air containing 10% water vapor for 2 h, and then introduced air for 2 h. After the calcination, the temperature was naturally cooled to room temperature to obtain 5% RuO2 / CeZrO x catalyst.

[0030] A method for preparing vinyl sulfate comprises the following steps:

[0031] 1g 5%RuO2 / CeZrO x Catalyst, 100g vinyl sulfite, 500g ethylene dichloride and 50g water were added to an enameled reactor. The temperature was controlled at 30°C. 2MPa of high-purity oxygen (content greater than 99.999%) was introduced. The reaction was continued for 5h. The mixture was filtered, cleaned and impurities removed to obtain vinyl sulfate. The catalyst was cleaned and dried and reused.

[0032] Example 2

[0033] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0034] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0035] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0036] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% potassium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0037] (2) The above ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and then filtered and washed to remove impurity ions to obtain Ru(OH)3 / CeZrOx slurry.

[0038] (3) The obtained Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the slurry was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0039] A method for preparing vinyl sulfate comprises the following steps:

[0040] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0041] Example 3

[0042] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0043] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0044] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0045] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0046] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0047] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0048] A method for preparing vinyl sulfate comprises the following steps:

[0049] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 40°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0050] Example 4

[0051] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0052] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0053] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0054] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0055] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0056] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0057] A method for preparing vinyl sulfate comprises the following steps:

[0058] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 50°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0059] Example 5

[0060] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0061] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0062] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0063] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0064] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0065] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0066] A method for preparing vinyl sulfate comprises the following steps:

[0067] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 3MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0068] Example 6

[0069] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0070] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0071] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0072] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0073] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0074] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0075] A method for preparing vinyl sulfate comprises the following steps:

[0076] Add 1g of 5% RuO2 / CeZrOx catalyst, 50g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0077] Example 7

[0078] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0079] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0080] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0081] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0082] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0083] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0084] A method for preparing vinyl sulfate comprises the following steps:

[0085] Add 1g of 5% RuO2 / CeZrOx catalyst, 150g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0086] Example 8

[0087] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0088] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0089] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0090] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0091] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (40% CeO2 / 60% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0092] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0093] A method for preparing vinyl sulfate comprises the following steps:

[0094] Add 1g of 5% RuO2 / CeZrOx catalyst, 200g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0095] Example 9

[0096] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0097] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0098] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0099] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0100] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (20% CeO2 / 80% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0101] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0102] A method for preparing vinyl sulfate comprises the following steps:

[0103] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0104] Example 10

[0105] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0106] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0107] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0108] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0109] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (60% CeO2 / 40% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0110] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0111] A method for preparing vinyl sulfate comprises the following steps:

[0112] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 30°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0113] Embodiment 11

[0114] A catalyst for synthesizing vinyl sulfate, wherein the catalyst is a supported catalyst, the supported catalyst is a RuO2 / CeZrOx catalyst, and the mass content of ruthenium in the catalyst is 5%;

[0115] The catalyst is used for catalytic synthesis of vinyl sulfate, and the catalyst exists in solid form during the process of catalytic synthesis of vinyl sulfate.

[0116] The preparation method of RuO2 / CeZrOx catalyst comprises the following steps:

[0117] (1) adding 1 g of ruthenium trichloride solid to 40 g of deionized water, stirring and dissolving for 10 min, adding 10% sodium hydroxide solution, adjusting the pH of the solution to 12, and continuing stirring for 30 min to obtain a ruthenium hydroxide alkaline solution;

[0118] (2) The above-mentioned ruthenium hydroxide alkaline solution was added dropwise to 20 g of cerium-zirconium composite oxide (60% CeO2 / 40% ZrO2) powder, and the mixture was stirred for 1 hour. The mixture was allowed to stand overnight, and the impurity ions therein were filtered and cleaned to obtain Ru(OH)3 / CeZrOx slurry.

[0119] (3) The Ru(OH)3 / CeZrOx slurry was dried at 100°C for 2 h, calcined at 450°C, and firstly, air containing 10% water vapor was introduced for 2 h, and then air was introduced for 2 h. After the calcination, the mixture was naturally cooled to room temperature to obtain a 5% RuO2 / CeZrOx catalyst.

[0120] A method for preparing vinyl sulfate comprises the following steps:

[0121] Add 1g of 5% RuO2 / CeZrOx catalyst, 100g of vinyl sulfite, 500g of ethylene dichloride and 50g of water into an enameled reactor, control the temperature at 55°C, introduce 2MPa of high-purity oxygen, react for 5h, filter, wash and remove impurities to obtain vinyl sulfate, wash and dry the catalyst and reuse it.

[0122] The RuO2 / CeZrOx catalyst in Example 1-11 was used to catalyze the synthesis of vinyl sulfate. The yields of vinyl sulfate when the catalyst was used for the first time and for the 10th time were shown in Table 1.

[0123] Table 1 Comparison of the yield of vinyl sulfate in the first use and 10 applications of the catalyst in Examples 1-11

[0124]

[0125] As can be seen from Table 1, after the RuO2 / CeZrOx catalyst prepared in the present application is used 10 times, the yield of vinyl sulfate is slightly reduced compared to when the catalyst is first used for catalytic synthesis of vinyl sulfate, but the yield of vinyl sulfate can still be higher than 90%, which shows that the catalyst has high catalytic activity, good stability, high yield for catalytic synthesis of vinyl sulfate, and can be recycled many times. The present invention uses the RuO2 / CeZrOx catalyst for catalytic synthesis of vinyl sulfate, which can greatly reduce the use of the precious metal Ru, thereby reducing production costs. The supported ruthenium catalyst of the present invention is used for catalytic synthesis of vinyl sulfate, and the synthesis process is green and environmentally friendly.

[0126] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing vinyl sulfate, It is characterized in that The following steps are involved: 1g RuO 2 / CeZrOx catalyst, 10-100g vinyl sulfite, 1-1000g ethylene dichloride and 1-500g water are added into a reaction kettle, and an oxidant of 0.1-6MPa is introduced, and the reaction is carried out at 10-80°C for 5h, and then filtered, washed and impurities are removed to obtain vinyl sulfate; The oxidant is high-purity oxygen or O 3 ; The RuO 2 / CeZrOx catalyst is a supported catalyst, and the mass content of ruthenium in the catalyst is 5%-10%; In the process of catalytic synthesis of vinyl sulfate, the catalyst is present in solid form; The mass content of cerium oxide in the cerium-zirconium composite oxide CeZrOx is 0.1%-90%.

2. The method for preparing vinyl sulfate according to claim 1, It is characterized in that The RuO 2 The preparation of / CeZrOx catalyst includes the following steps: (1) adding ruthenium trichloride solid to 20-60 g of deionized water, stirring to dissolve, then adding alkaline solution, adjusting the pH value of the solution to 10-14, and continuing to stir to obtain ruthenium hydroxide alkaline solution; (2) The above ruthenium hydroxide alkaline solution was added dropwise to the cerium-zirconium composite oxide powder, and the mixture was stirred for 1 hour, allowed to stand overnight, and filtered and washed to remove impurity ions to obtain Ru(OH) 3 / CeZrOx slurry; (3) The obtained Ru(OH) 3 / CeZrOx slurry is dried at 50-150℃ for 1-5h, calcined at 300-500℃, firstly introduced air containing 1-15% water vapor for 1-5h, then introduced air for 1-2h, and naturally cooled to room temperature after calcination to obtain RuO 2 / CeZrOx catalyst.

3. The method for preparing vinyl sulfate according to claim 2, It is characterized in that The solute in the alkaline solution in step (1) includes one or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.