A method for preparing a Cu-Ce catalyst with a multi-porous structure
Through the preparation method of the multi-channel structure Cu-Ce catalyst, the problem of poor catalytic toluene oxidation of existing catalysts is solved, and the efficient catalytic activity and catalyst purity are improved. The T90 temperature of the catalyst is reduced to below 260℃, ensuring that The efficiency and stability of the catalyst.
Patent Information
- Application Number
- CN202310038639.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-01-13
AI Technical Summary
The existing Cu-Ce catalysts have poor catalytic effects in the oxidation of volatile organic matter such as toluene, and it is difficult to maintain the purity and structural stability of the catalyst.
The Cu-Ce catalyst preparation method is adopted to form a Cu-Ce catalyst rich in pore structure by immersing, absorbing, heating, curing and stirring in Cu-Ce solution through degreasing cotton templates, forming a Cu-Ce catalyst rich in pore structure to ensure uniformity of Cu and Ce oxides. Dispersed and high purity.
The oxidation effect of the catalyst on toluene is significantly improved and the catalytic activity is improved. The T90 of the catalyst (temperature at 90% toluene conversion) is maintained below 260°C, ensuring the efficiency and stability of the catalyst.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0004163601790000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of Cu-Ce catalyst preparation methods, and in particular to a method for preparing a Cu-Ce catalyst with a multi-porous structure. Background Art
[0002] Volatile organic compounds, abbreviated as VOCs, refer to various organic compounds with a boiling point of 50°C to 260°C at room temperature. In my country, VOCs refer to organic compounds with a saturated vapor pressure greater than 70Pa at room temperature and a boiling point below 260°C at normal pressure, or all organic compounds with a vapor pressure greater than or equal to 10Pa and volatility at 20°C. Volatile organic compounds (VOCs) are precursors of PM2.5 and ozone. Controlling VOCs is of great significance to strengthening the coordinated control of PM2.5 and ozone, achieving synergistic effects in reducing pollution and carbon emissions, and promoting continuous improvement of ecological environment quality.
[0003] There are many existing methods for removing VOCs, such as adsorption, high-temperature pyrolysis, catalytic oxidation, photocatalytic degradation, low-temperature plasma removal technology, etc. Among them, catalytic oxidation is considered to be one of the most effective methods for removing VOCs. The key to the effectiveness of catalytic oxidation lies in the catalytic effect of the catalyst. As a highly efficient catalyst, Cu-Ce catalyst is widely used in the catalytic oxygen treatment of volatile organic matter represented by toluene. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a Cu-Ce catalyst with a multi-porous structure. The prepared Cu-Ce catalyst has a rich pore structure and has a better catalytic oxidation effect on volatile organic compounds such as toluene.
[0005] The above object of the present invention is achieved by the following technical solution: A method for preparing a multi-porous structure Cu-Ce catalyst comprises the following steps:
[0006] Step S1, preparation of absorbent cotton template:
[0007] Add absorbent cotton into the container, and then add sufficient anhydrous ethanol into the container so that the anhydrous ethanol can completely immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the anhydrous ethanol in the container;
[0008] Add enough deionized water to the container so that the deionized water can immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the deionized water in the container, and repeat this process 3-4 times; after drying the absorbent cotton, obtain an absorbent cotton template for later use;
[0009] Step S2, immersion reaction experiment: take an appropriate amount of Cu-Ce solution and add it into a container, the Cu-Ce solution is a mixed solution of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O, wherein the molar concentration of Cu(NO3)2·3H2O is 0.06mol / L-0.10mol / L; the molar concentration of Ce(NO3)3·6H2O is 0.15mol / L-0.54mol / L;
[0010] Add the absorbent cotton template prepared in step S1 to the Cu-Ce solution, adding 1 g of the absorbent cotton template for every 20-30 mL; immerse and absorb the absorbent cotton template in the Cu-Ce solution at room temperature for 22-26 hours;
[0011] The soaked absorbent cotton template and the Cu-Ce solution are placed in an environment of 60-100°C, and then NH3·H2O solution is added to react for 2-4 hours; wherein the molar ratio of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution is (1-1.4):1; after the reaction is completed, the absorbent cotton template is taken out from the reaction solution;
[0012] Step S3, cleaning and drying the absorbent cotton template: filtering the absorbent cotton template after the reaction in step S2 with deionized water, and then drying the absorbent cotton template;
[0013] Step S4, calcining the absorbent cotton template: placing the absorbent cotton dried in step S3 in an environment of 400-500° C. and calcining for 2-4 hours, and then taking out the calcined ash;
[0014] Step S5, catalyst separation: the ash calcined in step S4 is placed in a container, and sufficient deionized water is added to the container to form a mixed solution; the mixed solution is stirred at a stirring rate of 1000-1200 rpm for 30-50 minutes, and then the mixture is allowed to stand, and when the mixed solution is separated into layers, the upper layer of the separated layers is removed;
[0015] Repeat the steps of adding deionized water, stirring, and separating the upper layer of liquid for 3-5 times, with the standing time decreasing successively each time, and separating when the upper layer of liquid in the container is layered; filtering and removing the precipitate in the container, and obtaining the Cu-Ce catalyst after drying;
[0016] Step S6, catalyst calcination: the Cu-Ce catalyst obtained in step S5 is placed in a 400-500° C. environment and calcined for 2-4 hours, and then taken out and naturally cooled to obtain the multi-porous structure Cu-Ce catalyst.
[0017] Through the above technical scheme, the absorbent cotton has a rich fiber structure. Before using the absorbent cotton as a template, the absorbent cotton is first fully soaked with anhydrous ethanol to remove organic impurities in the absorbent cotton, thereby avoiding the adverse effects of impurities on the catalyst structure; the absorbent cotton has good water absorption. When the absorbent cotton template is immersed in a mixed solution of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O, the absorbent cotton template can well absorb the salt solution of Cu and Ce, so that the Cu and Ce oxides are evenly dispersed on the surface of the fiber structure. The Cu and Ce oxides attached to the absorbent cotton contain a large number of vacancies and defect structures, which are due to the strong interaction between Cu and Ce and the Cu + +Ce 4+ →Cu 2+ +Ce 3+ The invention discloses a method for removing the ashes from the burned absorbent cotton by stirring and utilizing the different settling rates of the catalyst and the ashes in water, thereby being able to separate and remove the impurities from the burned absorbent cotton well and ensure the purity of the Cu-Ce catalyst.
[0018] Preferably, in step S2, the molar ratio of NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution is 1:1.
[0019] Preferably, in step S2, the reaction time of adding NH3·H2O solution to the Cu-Ce solution is 4 hours.
[0020] Preferably, in step S2, the NH3·H2O solution is added in equal amounts in 3-5 times, and the time interval between each addition is equal. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which constitute a part of the specification, illustrate embodiments of the present invention and, together with the description, serve to explain the principles of the present invention.
[0022] Figure 1 This is the toluene conversion rate-temperature curve under the action of Cu-Ce catalyst sample. DETAILED DESCRIPTION
[0023] Example
[0024] Example 1
[0025] A method for preparing a Cu-Ce catalyst with a multi-porous structure comprises the following steps:
[0026] Step S1, preparation of absorbent cotton template:
[0027] Add absorbent cotton into the container, and then add sufficient anhydrous ethanol into the container so that the anhydrous ethanol can completely immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the anhydrous ethanol in the container;
[0028] Add enough deionized water to the container so that the deionized water can immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the deionized water in the container, and repeat this process 3-4 times; after drying the absorbent cotton, obtain an absorbent cotton template for later use;
[0029] Step S2, immersion reaction experiment; taking an appropriate amount of Cu-Ce solution and adding it into a container, the Cu-Ce solution is a mixed solution of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O, wherein the molar concentration of Ce(NO3)3·6H2O is 0.06mol / L-0.10mol / L; the molar concentration of Ce(NO3)3·6H2O is 0.15mol / L-0.54mol / L;
[0030] Add the absorbent cotton template prepared in step S1 to the Cu-Ce solution, adding 1 g of the absorbent cotton template for every 20-30 mL; immerse and absorb the absorbent cotton template in the Cu-Ce solution at room temperature for 22-26 hours;
[0031] The soaked absorbent cotton template and the Cu-Ce solution are placed in an environment of 60-100°C for 4 hours, and an equal amount of NH3·H2O solution is added in 3-5 times, with the time interval of each addition being the same; wherein the molar ratio of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution is 1:1; after the reaction is completed, the absorbent cotton template is taken out from the reaction solution;
[0032] Step S3, cleaning and drying the absorbent cotton template: filtering the absorbent cotton template after the reaction in step S2 with deionized water, and then drying the absorbent cotton template;
[0033] Step S4, calcining the absorbent cotton template: placing the absorbent cotton dried in step S3 in an environment of 400-500° C. and calcining for 2-4 hours, and then taking out the calcined ash;
[0034] Step S5, catalyst separation: the ash calcined in step S4 is placed in a container, and sufficient deionized water is added to the container to form a mixed solution; the mixed solution is stirred at a stirring rate of 1000-1200 rpm for 30-50 minutes, and then the mixture is allowed to stand, and when the mixed solution is separated into layers, the upper layer of the separated layers is removed;
[0035] Repeat the steps of adding deionized water, stirring, and separating the upper layer of liquid for 3-5 times, with the standing time decreasing successively each time, and separating when the upper layer of liquid in the container is layered; filtering and removing the precipitate in the container, and obtaining the Cu-Ce catalyst after drying;
[0036] Step S6, catalyst calcination: the Cu-Ce catalyst obtained in step S5 is placed in a 400-500° C. environment and calcined for 2-4 hours, and then taken out and naturally cooled to obtain the multi-porous structure Cu-Ce catalyst.
[0037] Example 2-3
[0038] The preparation methods of Examples 2 and 3 are the same as those of Example 1, except that in step S2, the molar ratios of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution are 1:1.2 and 1:1.4, respectively.
[0039] Embodiment 4-5
[0040] The preparation methods of Examples 4 and 5 are the same as those of Example 1, except that, in step S2, the reaction time of adding NH 3 ·H 2 O solution into the Cu—Ce solution is 3 hours and 2 hours respectively.
[0041] Example 6
[0042] A method for preparing a Cu-Ce catalyst with a multi-porous structure comprises the following steps:
[0043] Step S1, preparation of absorbent cotton template:
[0044] Add absorbent cotton into the container, and then add sufficient anhydrous ethanol into the container so that the anhydrous ethanol can completely immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the anhydrous ethanol in the container;
[0045] Add enough deionized water to the container so that the deionized water can immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the deionized water in the container, and repeat this process 3-4 times; after drying the absorbent cotton, obtain an absorbent cotton template for later use;
[0046] Step S2, immersion reaction experiment; taking an appropriate amount of Cu-Ce solution and adding it into a container, the Cu-Ce solution is a mixed solution of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O, wherein the molar concentration of Ce(NO3)3·6H2O is 0.06mol / L-0.10mol / L; the molar concentration of Ce(NO3)3·6H2O is 0.15mol / L-0.54mol / L;
[0047] Add the absorbent cotton template prepared in step S1 to the Cu-Ce solution, adding 1 g of the absorbent cotton template for every 20-30 mL; immerse and absorb the absorbent cotton template in the Cu-Ce solution at room temperature for 22-26 hours;
[0048] The soaked absorbent cotton template and the Cu-Ce solution are placed in an environment of 60-100°C for 4 hours, and an equal amount of NH3·H2O solution is added in 3-5 times, with the time interval of each addition being the same; wherein the molar ratio of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution is 1:1; after the reaction is completed, the absorbent cotton template is taken out from the reaction solution;
[0049] Step S3, cleaning and drying the absorbent cotton template: filtering the absorbent cotton template after the reaction in step S2 with deionized water, and then drying the absorbent cotton template;
[0050] Step S4, calcining the absorbent cotton template: placing the absorbent cotton dried in step S3 in an environment of 400-500° C. and calcining for 2-4 hours, and then taking out the calcined ash;
[0051] Step S5, catalyst separation: the ash calcined in step S4 is placed in a container, and sufficient deionized water is added to the container to form a mixed solution; the mixed solution is stirred at a stirring rate of 1000-1200 rpm for 30-50 minutes, and then the mixture is allowed to stand, and when the mixed solution is separated into layers, the upper layer of the separated layers is removed;
[0052] The steps of adding deionized water, stirring, and separating the upper liquid are repeated 3-5 times, with the standing time decreasing successively each time, and separation is performed when the upper liquid in the container is stratified; the precipitate in the container is filtered out and dried to obtain the Cu-Ce catalyst.
[0053] Embodiment 7-8
[0054] The preparation methods of Examples 7 and 8 are the same as those of Example 6, except that in step S2, the molar ratios of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution are 1.2:1 and 1.4:1, respectively.
[0055] Comparative Example 1
[0056] A method for preparing a Cu-Ce catalyst comprises the following steps:
[0057] Cerium nitrate was dissolved and dispersed in an aqueous solution to form a 0.4 mol / L cerium nitrate solution, to which a 6 mol / L sodium hydroxide solution was added dropwise, maintaining a molar ratio of metal to sodium hydroxide of 1:105, and the stirring time was continued for 0.5 h. The mixture was fully mixed and reacted, and the mixed solution was transferred to a 100 mL high-pressure reactor, reacted at 100 ° C for 24 h, cooled, centrifuged and washed, dried in an oven at 60 ° C for 24 h, and calcined in an air atmosphere at 400 ° C for 4 h, with a heating rate of 2 ° C / min, to obtain a rod-shaped CeO2 carrier. Take 1g of carrier CeO2 and dissolve it in aqueous solution, select Cu(NO3)2 as the precursor salt, keep the CuO loading at 20wt% / g carrier, then add citric acid solution, control the molar ratio of citric acid to metal to be 1:1, stir at room temperature for 1h, then put it into a vacuum drying oven, dry it at 70℃ to remove excess water, form a colloidal substance, continue to increase the temperature to 100℃, dry it for 10h, use a two-stage calcination method, calcine at 300℃ in an air atmosphere for 2h, program the temperature to 400℃ and calcine for 2h, with a heating rate of 1℃ / min, to obtain a Cu-Ce catalyst with a nanorod structure, and prepare catalyst A.
[0058] The above method is excerpted from the Chinese invention patent application with application number CN201810337489.X, entitled A nanorod-structured Cu-Ce catalyst for NH3 catalytic oxidation, preparation method and application.
[0059] Comparative Example 2
[0060] A method for preparing a Cu-Ce catalyst comprises the following steps:
[0061] Add 6g of P123 (polyethylene oxide-polyethylene oxide-polyethylene oxide triblock copolymer, number average molecular weight 5800) to a mixed solution of 220g of deionized water and 12g (35wt%) concentrated hydrochloric acid. Stir for 6 hours until P123 is completely dissolved to form a transparent colloidal solution. Then add 6g of n-butanol, continue stirring for 1 hour, then add 12.86g of tetraethyl orthosilicate, and continue stirring for 24 hours. Then move the mixed solution into a reactor and hydrothermally react at 100°C for 24 hours. After filtering, washing, and drying, the obtained sample is calcined at 550°C in a muffle furnace under air atmosphere for 4 hours to obtain a white powder, which is mesoporous silicon KIT-6;
[0062] 2.2gCe(NO3)3·6H2O, 0.21gCu(NO3)2·3H2O and 0.22gKNO3 (wherein the molar percentage of Cu / (Cu+Ce) is 15% and the molar ratio of (Cu+Ce) / K is 2) are dissolved in 10mL of ethanol solution and stirred for 20min to completely dissolve. The final solution concentration is about 0.4mol / L. Then 1g of mesoporous silicon KIT-6 is added to the mixed solution, heated and stirred at 60℃ in a water bath until the solution is completely volatilized to form a dry powder. The powder is heated to 450℃ at a heating rate of 1℃min-1 in a muffle furnace air atmosphere and maintained for 4h to form a composite powder material of mesoporous silicon and metal oxide. Then the powder material is stirred in a 60℃ hot KOH (1mol / L) solution for 1h, repeated twice, and washed and dried to obtain a copper-cerium catalyst with a double-channel three-dimensional structure.
[0063] The above method is excerpted from the Chinese invention patent application with application number CN201610651256.8, entitled Preparation process of copper-cerium catalyst with double-channel three-dimensional structure and its products.
[0064] Test methods
[0065] The Cu-Ce catalyst samples prepared in Examples 1 to 8 and the Cu-Ce catalyst samples prepared in Comparative Examples 1-2 were tested according to the following method.
[0066] A 100 mg Cu-Ce catalyst sample was taken and placed in a fixed bed tubular reactor. The reaction gas was introduced into the fixed bed tubular reactor, wherein the reaction gas included (the toluene concentration in the introduced gas was 1000 pmm, the volume fraction of oxygen was 20%, and nitrogen served as a balance gas), the gas air flow rate was 60000 ml / (gh), and the total gas flow rate was 100 ml / min.
[0067] The reaction temperature of the fixed-bed tubular reactor changes according to the following rule: first heat up to 120°C and stabilize for 30 minutes; then heat up to 140°C and stabilize for 5 minutes; then heat up to 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, and 300°C in sequence, stabilize at each temperature point for 5 minutes, and repeat the test three times at each temperature point.
[0068] The concentrations of toluene and carbon dioxide in the outlet gas of the fixed bed tubular reactor were detected by a flame ionization detector and a thermal conductivity detector. The reaction temperature T was set at 50% and 90% when the toluene conversion rate was 50%. 50 and T 90 To evaluate the catalytic activity of the samples.
[0069] The toluene conversion rate is calculated by formula (1):
[0070]
[0071] Where: C toluene is the toluene conversion rate, %; [C7H8] in is the concentration of toluene in the inlet gas, ppm; [C7H8] out is the concentration of toluene in the outlet gas, ppm.
[0072] The test results are shown in Table 1 and Figure 1 shown.
[0073]
[0074] Table 1 Test data of catalytic activity of Cu-Ce catalyst samples
[0075] From Table 1 and Figure 1 We can get:
[0076] The catalyst prepared by the present invention has a high catalytic activity. 90 (The temperature corresponding to 90% toluene conversion) was kept below 260°C. The reaction time and the amount of precipitant used will affect the catalyst activity. The catalyst T corresponding to the preparation conditions in Example 1 90 The minimum is 239° C. The activity of Example 6-8, which was not further calcined after impurity removal, was lower than that of the calcined catalyst.
[0077] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A method for preparing a multi-porous Cu-Ce catalyst for catalytic oxidation of volatile organic compounds, characterized in that: The following steps are involved: Step S1, preparation of absorbent cotton template: Add absorbent cotton into the container, and then add sufficient anhydrous ethanol into the container so that the anhydrous ethanol can completely immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the anhydrous ethanol in the container; Add enough deionized water to the container so that the deionized water can immerse the absorbent cotton in the container; after immersing the absorbent cotton for 1-2 hours, remove the deionized water in the container, and repeat this process 3-4 times; after drying the absorbent cotton, obtain an absorbent cotton template for later use; Step S2, immersion reaction experiment: take an appropriate amount of Cu-Ce solution and add it into a container, the Cu-Ce solution is a mixed solution of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O, wherein the molar concentration of Cu(NO3)2·3H2O is 0.06mol / L-0.10mol / L; the molar concentration of Ce(NO3)3·6H2O is 0.15mol / L-0.54mol / L; Add the absorbent cotton template prepared in step S1 to the Cu-Ce solution, adding 1 g of the absorbent cotton template for every 20-30 mL; immerse and absorb the absorbent cotton template in the Cu-Ce solution at room temperature for 22-26 hours; The soaked absorbent cotton template and the Cu-Ce solution are placed in an environment of 60-100°C, and then NH3·H2O solution is added to react for 2-4 hours; wherein the molar ratio of the added NH3·H2O to the sum of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O in the Cu-Ce solution is (1-1.4):1; after the reaction is completed, the absorbent cotton template is taken out from the reaction solution; the NH3·H2O solution is added in equal amounts in 3-5 times, and the time interval between each addition is equal; Step S3, cleaning and drying the absorbent cotton template: filtering the absorbent cotton template after the reaction in step S2 with deionized water, and then drying the absorbent cotton template; Step S4, calcining the absorbent cotton template: placing the absorbent cotton dried in step S3 in an environment of 400-500° C. and calcining for 2-4 hours, and then taking out the calcined ash; Step S5, catalyst separation: the ash calcined in step S4 is placed in a container, and sufficient deionized water is added to the container to form a mixed solution; the mixed solution is stirred at a stirring rate of 1000-1200 rpm for 30-50 minutes, and then the mixture is allowed to stand, and when the mixed solution is separated into layers, the upper layer of the separated layers is removed; Repeat the steps of adding deionized water, stirring, and separating the upper layer of liquid for 3-5 times, with the standing time decreasing successively each time, and separating when the upper layer of liquid in the container is layered; filtering and removing the precipitate in the container, and obtaining the Cu-Ce catalyst after drying; Step S6, catalyst calcination: the Cu-Ce catalyst obtained in step S5 is placed in a 400-500° C. environment and calcined for 2-4 hours, and then taken out and naturally cooled to obtain the multi-porous structure Cu-Ce catalyst.
2. The method according to claim 1, characterized in that: In step S2, the molar ratio of NH3.H2O to the sum of Cu(NO3)2.3H2O and Ce(NO3)3.6H2O in the Cu-Ce solution is 1:
1.
3. The method according to claim 1, characterized in that: In step S2, the reaction time of adding NH3·H2O solution to the Cu-Ce solution is 4 hours.