A method for preparing titanium oxide coated diamond powder

By carrying out Ti(SO4)2 crystallization and thermal decomposition reactions at ultra-low temperatures, the problem of high cost and long time for coating titanium oxide on the surface of diamond powder is solved, a high-stability and low-cost titanium oxide coating layer is achieved, and the Performance and stability of diamond/metal composites.

CN116375024BActive Publication Date: 2024-10-11KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310271769.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-11
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

In the preparation process of composite materials with diamond as reinforcement, carbon atoms on the surface of diamond powder are easy to diffuse under high-temperature sintering conditions, affecting material properties. The existing titanium oxide coating process is costly or takes a long time and is prone to defects.

Method used

By preparing a saturated ethanol solution of Ti(SO4)2 containing diamond powder at room temperature, and performing magnetic stirring at ultra-low temperatures of -50°C to -100°C, Ti(SO4)2 crystallizes and precipitates on the surface of the diamond powder, combined with thermal decomposition reaction to prepare titanium oxide-coated diamond powder, simplifying the process and reducing costs.

Benefits of technology

It achieves high stability of the titanium oxide coating layer, improves the performance and stability of the diamond/metal composite material, has a simple process and low cost, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004134971240000031
    Figure BDA0004134971240000031
  • Figure BDA0004134971240000033
    Figure BDA0004134971240000033
  • Figure BDA0004134971240000034
    Figure BDA0004134971240000034
Patent Text Reader

Abstract

The invention discloses a method for preparing titanium oxide-coated diamond powder, and belongs to the field of diamond powder surface treatment. The method of the invention is as follows: pre-treated diamond powder and Ti(SO4)2 are placed in ethanol and subjected to magnetic stirring to obtain a Ti(SO4)2 ethanol saturated solution containing diamond powder; the mixed solution is placed in a low temperature thermostat, cooled to an ultra-low temperature of ‑50°C to ‑100°C, and then subjected to magnetic stirring to greatly reduce the solubility of Ti(SO4)2 in ethanol and crystallize on the surface of the diamond powder; the mixed solution is filtered and separated at ultra-low temperature to obtain diamond powder coated with a Ti(SO4)2 film on the surface; the diamond powder coated with the Ti(SO4)2 film is heated to 500‑600°C to decompose Ti(SO4)2 into TiO2 to obtain diamond powder coated with a TiO2 film on the surface. The present invention realizes coating titanium oxide on the surface of micron diamond powder through a physical method of ultra-low temperature crystallization of Ti(SO4)2 combined with a subsequent thermal decomposition reaction, which can reduce the use of Ti(SO4)2 raw materials, has the characteristics of simple process and low cost, and can be industrially applied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for preparing titanium oxide coated diamond powder, and belongs to the field of diamond powder surface treatment. Background Art

[0002] Diamond is widely used as a reinforcement in the preparation of composite materials due to its high hardness, high strength, friction and wear resistance, and low thermal expansion coefficient. However, during the preparation of composite materials with diamond as reinforcement, the carbon atoms on the surface of diamond powder are easy to diffuse into the matrix and react with the matrix under high-temperature sintering conditions, thereby affecting the performance of the composite material. Titanium oxide is an ideal coating material for diamond surface passivation treatment due to its stable chemical properties and high temperature resistance. By plating titanium oxide on the surface of diamond powder, the performance and stability of diamond / metal composite materials can be improved.

[0003] At present, the titanium dioxide surface treatment processes for diamond powder mainly include vacuum plating and sol-gel method. The National Institute of Nanotechnology and Engineering uses vacuum plating to obtain titanium dioxide thin film. The process is carried out in a pulsed sputtering vacuum plating device. With metal titanium as the target material, oxygen and argon are filled into the vacuum chamber and a pulse power supply is used to glow discharge in the vacuum chamber to make metal titanium react with oxygen to obtain a titanium dioxide thin film; Shenyang University of Technology uses the sol-gel method to prepare titanium dioxide thin film. The process is: first, anhydrous ethanol, tetrabutyl titanate and organic chelating agent are stirred and evenly mixed to form a tetrabutyl titanate ethanol complex solution, and ethanol aqueous solution and non-ionic surfactant are added to the complex solution. Stir until a titanium dioxide sol is obtained, and then the film is plated and calcined after static aging. Titanium dioxide thin films can be prepared on substrates of different shapes. The titanium dioxide thin film obtained by vacuum plating has good uniformity, but the cost is high; the sol-gel process takes a long time (often several days or weeks), and is prone to defects such as micropores. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing titanium oxide coated diamond powder, wherein a saturated Ti(SO4)2 ethanol solution containing diamond powder prepared at room temperature is placed in an ultra-low temperature of -50°C to -100°C. Since the freezing point of ethanol (-114.1°C) is low and the solubility of Ti(SO4)2 in room temperature and ultra-low temperature ethanol is quite different, Ti(SO4)2 is precipitated in large quantities on the surface of the diamond powder, thereby reducing the use of the raw material Ti(SO4)2. Diamond powder coated with titanium oxide is obtained by a physical method of ultra-low temperature crystallization of Ti(SO4)2 and in combination with a subsequent thermal decomposition reaction, which has the characteristics of simple process and low cost and can be industrially applied.

[0005] The method of the present invention specifically comprises the following steps:

[0006] (1) Pretreatment of diamond powder: Add diamond powder to HNO3 solution and stir it magnetically, then wash it repeatedly with deionized water until it becomes neutral, and then place it in a drying oven to dry for use.

[0007] (2) Obtaining a mixed solution: Prepare materials according to the ratio of diamond powder mass: titanium sulfate mass: ethanol mass = (25-30): (80-85): 100, add the pretreated diamond powder and Ti(SO4)2 into ethanol and stir magnetically for 20 minutes to obtain a saturated Ti(SO4)2 ethanol solution containing diamond powder.

[0008] (3) Ti(SO4)2 coated diamond powder: The mixed solution is placed in a low temperature thermostat, the temperature is lowered to an ultra-low temperature of -50°C to -100°C, and then magnetically stirred for 20-50 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and crystallize on the surface of the diamond powder. The mixed solution is filtered and separated at an ultra-low temperature to obtain diamond powder coated with a Ti(SO4)2 film.

[0009] (4) TiO2 coated diamond powder: Diamond powder coated with Ti(SO4)2 film is heated to 500°C-600°C and decomposed for 40-100 min to obtain diamond powder with TiO2 film coated on the surface.

[0010] Preferably, the concentration of the HNO3 solution in step (1) of the present invention is 0.5 to 3 mol / L, and the magnetic stirring time is 15 to 25 min.

[0011] Preferably, the particle size of the diamond powder of the present invention is 1-100 μm.

[0012] Preferably, the magnetic stirring time in step (2) of the present invention is 20 min.

[0013] Preferably, the magnetic stirring time in step (3) of the present invention is 20-50 min.

[0014] Principle of the invention:

[0015] (1) Principle of ultra-low temperature crystallization titanium sulfate plating

[0016] Ultra-low temperature crystallized titanium sulfate plating is carried out by adding pre-treated diamond powder and Ti(SO4)2 into ethanol (freezing point -114.1°C) at room temperature to obtain a Ti(SO4)2 ethanol saturated solution containing diamond powder; Figure 1 The solubility curve of Ti(SO4)2 in ethanol changes with temperature. Figure 1It can be seen that there is a large difference in the solubility of Ti(SO4)2 in ethanol at room temperature (20℃-30℃) and -100℃. Therefore, Ti(SO4)2 is dissolved in ethanol at room temperature (20℃-30℃), and the preferred cooling range is -50℃~-100℃.

[0017] (2) Principle of controlling the thickness of titanium oxide coating

[0018] Diamond powder and Ti(SO4)2 are added to ethanol in a ratio of diamond powder mass: titanium sulfate mass: ethanol mass = (25-30): (80-85): 100, and the solubility of Ti(SO4)2 in ultra-low temperature ethanol is reduced by adjusting the cooling temperature of the saturated Ti(SO4)2 ethanol solution containing diamond powder, so that Ti(SO4)2 crystallizes on the surface of diamond powder; Figure 1 The solubility curve of Ti(SO4)2 in ethanol with temperature and the fitting formula (1) can be used to calculate the solubility R of Ti(SO4)2 in ethanol at room temperature and ultra-low temperature. T :

[0019]

[0020] (1) Where, T is temperature, °C; R T —Solubility of Ti(SO4)2 in ethanol at T℃, g / 100g ethanol.

[0021] According to the difference in solubility of Ti(SO4)2 in room temperature and ultra-low temperature ethanol in formula (1), the precipitation mass M1 of Ti(SO4)2 on the surface of diamond powder can be obtained:

[0022] M1=R T1 -R T2 (2)

[0023] (2) Where M1 is the mass of Ti(SO4)2 precipitated on the surface of diamond powder, g / 100 g ethanol;

[0024] R T1 —Solubility of Ti(SO4)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Ti(SO4)2 in ultra-low temperature ethanol, g / 100g ethanol.

[0025] The chemical equation for the thermal decomposition reaction of Ti(SO4)2 is as follows:

[0026]

[0027] According to the relative molecular mass ratio of Ti(SO4)2 and TiO2 in formula (2) and (3), the mass M2 of TiO2 obtained after thermal decomposition of Ti(SO4)2 can be obtained:

[0028]

[0029] M2=0.33(R T1 -R T2 ) (4)

[0030] In formula (4), M1 is the mass of Ti(SO4)2 precipitated on the surface of diamond powder, g / 100g ethanol;

[0031] M2—mass of TiO2 from thermal decomposition of Ti(SO4)2, g / 100g ethanol; R T1 —Solubility of Ti(SO4)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Ti(SO4)2 in ultra-low temperature ethanol, g / 100g ethanol.

[0032] According to the density formula, diamond powder particle size and mass, the surface area calculation formula of diamond powder can be obtained:

[0033]

[0034] In formula (5), S is the surface area of ​​diamond powder, cm 2 ;ρ1—density of diamond powder, ρ1=3.52 g / cm 3 ; m—mass of diamond powder, g / 100g ethanol; r—particle size of diamond powder, μm.

[0035] According to the ratio of diamond powder mass: titanium sulfate mass: ethanol mass = (25-30): (80-85): 100 and combined with equations (1), (2), (4) and (5), according to the molecular weight of the reactants, the thickness calculation equation (6) of Ti(SO4)2 and the thickness calculation equation (7) of TiO2 can be derived:

[0036]

[0037]

[0038] In formulas (6)-(7), δ1 is the average thickness of Ti(SO4)2 coating, μm; δ2 is the average thickness of TiO2 coating, μm; S is the surface area of ​​diamond powder, cm 2; M1—mass of Ti(SO4)2 precipitated on the surface of diamond powder, g / 100g ethanol; M2—mass of TiO2 thermally decomposed from Ti(SO4)2, g / 100g ethanol; ρ1—density of diamond powder, ρ1=3.52g / cm 3 ;ρ2—density of Ti(SO4)2, ρ2=1.47g / cm 3 ;ρ3—density of TiO2, ρ3=4.26g / cm 3 ; m—mass of diamond powder, g / 100g ethanol; r—diamond powder particle size, μm; R T1 —Solubility of Ti(SO4)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Ti(SO4)2 in ultra-low temperature ethanol, g / 100g ethanol.

[0039] 3. Selection of heating decomposition temperature and time of Ti(SO4)2

[0040] At 400°C, Ti(SO4)2 begins to decompose into TiO2 due to heat. When the temperature rises to 500°C, Ti(SO4)2 is completely decomposed into TiO2. In order to obtain TiO2-coated diamond powder, the selected decomposition temperature is 500°C-600°C and the decomposition time is 40-100 minutes.

[0041] Beneficial effects of the present invention:

[0042] The present invention forms a saturated solution containing diamond powder by adding diamond powder and Ti(SO4)2 into ethanol, and then lowers the temperature to an ultra-low temperature of -50°C to -100°C, so that the solubility of Ti(SO4)2 in ethanol is greatly reduced and crystallized on the surface of the diamond powder. First, the freezing point of ethanol (-114.1°C) is low; second, there is a large difference in the solubility of Ti(SO4)2 in room temperature and ultra-low temperature ethanol. Through the physical method of ultra-low temperature crystallization of Ti(SO4)2 and in combination with the subsequent thermal decomposition reaction, the surface of micron diamond powder is coated with titanium oxide, which can reduce the use of Ti(SO4)2 raw materials; the formed titanium oxide coating layer has high stability, which can improve the performance and stability of composite materials such as diamond / aluminum; it has the characteristics of simple process and low cost, and can be industrially applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Process flow chart of diamond powder surface coating with titanium oxide.

[0044] Figure 2 The solubility curve of Ti(SO4)2 in ethanol changes with temperature. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the contents described above.

[0046] Example 1

[0047] A method for preparing titanium oxide-coated diamond powder comprises the following steps:

[0048] (1) Raw material pretreatment: Commercially available diamond powder with a particle size of 1 μm was added to a 0.5 mol / L HNO3 solution and magnetically stirred for 25 min. The powder was then repeatedly washed with deionized water until neutral and placed in a drying oven for drying.

[0049] (2) Obtaining a mixed solution: Prepare materials in a ratio of mass of diamond powder: mass of titanium sulfate: mass of ethanol = 30:80:100, add diamond powder and Ti(SO4)2 into ethanol at room temperature (20°C) and stir magnetically for 20 minutes to obtain a saturated ethanol solution of Ti(SO4)2 containing diamond powder.

[0050] (3) Ti(SO4)2 coated diamond powder: The mixed solution obtained in step (2) is placed in a low-temperature thermostat and the temperature is lowered to an ultra-low temperature of -50°C, followed by magnetic stirring for 50 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and allow crystallization on the surface of the diamond powder. The mixed solution is filtered and separated at an ultra-low temperature to obtain diamond powder coated with a 0.5 μm thick Ti(SO4)2 film on the surface.

[0051] (4) TiO2 coated diamond powder: The diamond powder coated with the Ti(SO4)2 film obtained in step (3) was heated to 600°C and decomposed for 40 minutes to obtain a diamond powder with a 0.1 μm thick TiO2 film coated on the surface.

[0052] Example 2

[0053] A method for preparing titanium oxide coated diamond powder, characterized in that it specifically comprises the following steps:

[0054] (1) Raw material pretreatment: Commercially available diamond powder with a particle size of 30 μm was added to a dilute HNO3 solution with a concentration of 1.2 mol / L and magnetically stirred for 22 min. The powder was then repeatedly washed with deionized water until neutral and placed in a drying oven for drying.

[0055] (2) Obtaining a mixed solution: Prepare materials in a ratio of mass of diamond powder: mass of titanium sulfate: mass of ethanol = 28:82:100, add diamond powder and Ti(SO4)2 into ethanol at room temperature (23°C) and stir magnetically for 20 minutes to obtain a saturated ethanol solution of Ti(SO4)2 containing diamond powder.

[0056] (3) Ti(SO4)2 coated diamond powder: The mixed solution obtained in step (2) is placed in a low-temperature thermostat and the temperature is lowered to an ultra-low temperature of -65°C, followed by magnetic stirring for 40 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and allow crystallization on the surface of the diamond powder. The mixed solution is filtered and separated at an ultra-low temperature to obtain diamond powder having a surface coated with a 21.0 μm thick Ti(SO4)2 film.

[0057] (4) TiO2 coated diamond powder: The diamond powder coated with the Ti(SO4)2 film obtained in step (3) was heated to 560°C and decomposed for 60 minutes to obtain a diamond powder with a 2.4 μm thick TiO2 film coated on the surface.

[0058] Example 3

[0059] A method for preparing titanium oxide coated diamond powder, characterized in that it specifically comprises the following steps:

[0060] (1) Raw material pretreatment: Commercially available diamond powder with a particle size of 60 μm was added to a dilute HNO3 solution with a concentration of 2.2 mol / L and magnetically stirred for 18 min. The powder was then repeatedly washed with deionized water until neutral and placed in a drying oven for drying.

[0061] (2) Obtaining a mixed solution: Prepare materials in a ratio of mass of diamond powder: mass of titanium sulfate: mass of ethanol = 27:83:100, add diamond powder and Ti(SO4)2 into ethanol at room temperature (27°C) and stir magnetically for 20 minutes to obtain a saturated ethanol solution of Ti(SO4)2 containing diamond powder.

[0062] (3) Ti(SO4)2 coated diamond powder: The mixed solution obtained in step (2) is placed in a low-temperature thermostat and the temperature is lowered to an ultra-low temperature of -85°C, followed by magnetic stirring for 30 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and allow crystallization on the surface of the diamond powder. The mixed solution is filtered and separated at an ultra-low temperature to obtain diamond powder coated with a 57.3 μm thick Ti(SO4)2 film on the surface.

[0063] (4) TiO2 coated diamond powder: The diamond powder coated with the Ti(SO4)2 film obtained in step (3) was heated to 530°C and decomposed for 80 minutes to obtain a diamond powder with a 6.5 μm thick TiO2 film coated on the surface.

[0064] Example 4

[0065] A method for preparing titanium oxide coated diamond powder, characterized in that it specifically comprises the following steps:

[0066] (1) Raw material pretreatment: Commercially available diamond powder with a particle size of 100 μm was added to a dilute HNO3 solution with a concentration of 3 mol / L and magnetically stirred for 15 min. The powder was then repeatedly washed with deionized water until neutral and placed in a drying oven for drying.

[0067] (2) Obtaining a mixed solution: Prepare materials in a ratio of mass of diamond powder: mass of titanium sulfate: mass of ethanol = 25:85:100, add diamond powder and Ti(SO4)2 into ethanol at room temperature (30°C) and stir magnetically for 20 minutes to obtain a saturated ethanol solution of Ti(SO4)2 containing diamond powder.

[0068] (3) Ti(SO4)2 coated diamond powder: The mixed solution obtained in step (2) is placed in a low-temperature thermostat and the temperature is lowered to an ultra-low temperature of -100°C and then magnetically stirred for 20 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and crystallize on the surface of the diamond powder. The mixed solution is filtered and separated at an ultra-low temperature to obtain diamond powder with a surface coated with a 122.6 μm thick Ti(SO4)2 film.

[0069] (4) TiO2 coated diamond powder: The diamond powder coated with the Ti(SO4)2 film obtained in step (3) was heated to 500°C and decomposed for 100 minutes to obtain a diamond powder with a 14.0 μm thick TiO2 film coated on the surface.

Claims

1. A method for preparing titanium oxide-coated diamond powder, characterized in that: The specific steps include: (1) Pre-treating the diamond powder: adding the diamond powder to the HNO3 solution and subjecting it to magnetic stirring, then repeatedly washing it with deionized water until it becomes neutral, and then placing it in a drying oven for drying; (2) Obtaining a mixed solution: preparing materials according to the ratio of diamond powder mass: titanium sulfate mass: ethanol mass = (25-30): (80-85): 100, adding the pretreated diamond powder and Ti(SO4)2 into ethanol and magnetically stirring for 20 minutes to obtain a Ti(SO4)2 ethanol saturated solution containing diamond powder; (3) Ti(SO4)2 coated diamond powder: Place the mixed solution in a low temperature thermostat, lower the temperature to -50℃~-100℃, and then stir it magnetically for 20-50 minutes to reduce the solubility of Ti(SO4)2 in ultra-low temperature ethanol and crystallize on the surface of diamond powder. Filter and separate the mixed solution at ultra-low temperature to obtain diamond powder coated with Ti(SO4)2 film. (4) TiO2 coated diamond powder: Diamond powder coated with Ti(SO4)2 film is heated to 500℃-600℃ and decomposed for 40-100min to obtain diamond powder with TiO2 film coated on the surface.

2. The method for preparing titanium oxide coated diamond powder according to claim 1, characterized in that: The concentration of the HNO3 solution in step (1) is 0.5-3 mol / L, and the magnetic stirring time is 15-25 min.

3. The method for preparing titanium oxide coated diamond powder according to claim 1 or 2, characterized in that: The particle size of the diamond powder is 1-100 μm.