A method for preparing low-calcium clinker by desulfurization of phosphogypsum
By designing appropriate raw material ratios and process flows, efficient desulfurization of phosphogypsum and low-calcium clinker production are achieved, solving the problems of phosphogypsum resource utilization and environmental pollution, and improving the application value of phosphogypsum in cement clinker.
Patent Information
- Application Number
- CN202310339927.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Phosphogypsum is a by-product produced in the process of producing phosphate fertilizer. The presence of fluorine and organic matter leads to resource waste and environmental pollution, and its desulfurization is difficult, resulting in low strength of phosphogypsum co-produced cement, making it difficult to replace limestone, increasing process costs and operational difficulty. .
Using low-cost conventional raw materials, drying, grinding, and making pellets are used for desulfurization. Combined with siliceous raw materials, they are calcined in a rotary kiln. The appropriate molar ratio and chemical composition ratio of carbon and phosphogypsum are designed to achieve efficient desulfurization. and low-energy, low-calcium clinker production.
The high-efficiency desulfurization rate of phosphogypsum (more than 99%) has been achieved, and environmentally friendly low-calcium clinker has been produced. The mineral composition is mainly C3S2 and CS, and the carbonization intensity is high, which reduces process costs and operation difficulty.
Smart Images

Figure CN116375365B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a method for preparing low-calcium clinker by desulfurization of phosphogypsum. Background Art
[0002] Phosphogypsum is a byproduct of phosphate fertilizer production. Its composition is complex. In addition to hydrated calcium sulfate, there are also incompletely decomposed phosphate rock, residual phosphoric acid, fluoride, acid insoluble matter, organic matter, etc. Among them, the presence of fluorine and organic matter has the greatest impact on the resource utilization of phosphogypsum. Stacking will occupy a large amount of land and cause pollution to water and land resources. At present, there is no better way to utilize phosphogypsum. Its resource utilization and safe and efficient utilization are of great significance to solving the problems of environmental pollution and resource waste caused by stacking.
[0003] Using phosphogypsum instead of limestone as a source of CaO to produce cement clinker can provide CaO in the clinker with phosphogypsum, which can process a large amount of phosphogypsum and reduce the mining of natural limestone mines. Both active admixtures and clinkers have strict requirements on the SO3 content, but CaSO4 requires a higher temperature to completely decompose and desulfurize compared to CaCO3, which will increase the difficulty and cost of the process operation. It can even still exist in large quantities under high-temperature calcination, which undoubtedly restricts the difficulty of applying phosphogypsum.
[0004] In 1969, the Austrian Linz Company completed and put into operation a plant for producing cement from phosphogypsum and sulfuric acid. In the 1980s, my country also built 7 sets of equipment. The main method is to dry and dehydrate the phosphogypsum, mix it with coke, clay, sandstone, etc. according to the clinker ratio, and calcine it in a hollow rotary kiln to produce clinker. The SO2 in the kiln gas is converted and absorbed to produce sulfuric acid. However, the strength of cement produced from phosphogypsum is generally low, and it even fails to reach the strength grade of 42.5 ordinary Portland cement. At present, most of the co-production units have been shut down.
[0005] There have been many literature reports on the research on the decomposition of phosphogypsum using carbonaceous raw materials, carbon monoxide atmosphere, elemental sulfur, etc., but it is difficult to achieve a desulfurization rate of more than 95% for phosphogypsum by relying solely on the reduction of carbon and sulfur. If the desulfurization rate does not meet this requirement, it will have many adverse effects on the production and application of clinker.
[0006] How to process phosphogypsum in large quantities to achieve better desulfurization effect and prepare environmentally friendly, low-energy-consuming, low-calcium clinker with high carbonization strength based on C3S2 and CS minerals as a composite system has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing low-calcium clinker by desulfurization of phosphogypsum, which adopts low-cost conventional raw materials, can process a large amount of phosphogypsum, so that the phosphogypsum can obtain a better desulfurization effect, and prepare environmentally friendly, low-energy-consuming, low-calcium clinker with high carbonization strength using C3S2 and CS minerals as a composite system.
[0008] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0009] A method for preparing low-calcium clinker by desulfurization of phosphogypsum comprises the following steps:
[0010] (1) obtaining phosphogypsum, carbonaceous raw materials, and silicon-aluminum-iron raw materials, drying, crushing, mixing, and grinding after mixing;
[0011] (2) adding water to the obtained mixture to form pellets, and drying;
[0012] (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4;
[0013] (4) After the desulfurized material is cooled, it is added to the siliceous raw material and mixed and ground so that its KH value and the mass ratio of total CaO to SiO2 in the chemical composition meet the requirements of the designed low-calcium clinker, and then enters the rotary kiln for calcination to obtain low-calcium clinker.
[0014] According to the above scheme, the carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.
[0015] According to the above scheme, the ferro-aluminum-silicon raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, and fly ash.
[0016] According to the above scheme, the ingredients used in step (1) are that the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6.
[0017] According to the above scheme, the diameter of the ball in step (2) is 1-3 cm.
[0018] According to the above scheme, the desulfurization temperature of the desulfurization furnace in step (3) is 1150-1250°C.
[0019] According to the above scheme, the siliceous raw material in step (4) is one or more of sandstone, coal gangue, silica, clay, fly ash and glass.
[0020] According to the above scheme, the KH value and the mass ratio of total CaO to SiO2 in the chemical composition in step (4) are 0.4-0.45 and 1.2-1.4 respectively.
[0021] According to the above scheme, the calcination temperature of the rotary kiln in step (4) is 1200-1300°C.
[0022] According to the above scheme, the mineral composition of the low-calcium clinker obtained in step (4) is mainly low-calcium minerals C3S2 and CS, wherein the content of C3S2 is 60-90% and the content of CS is 10-30%.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The invention can process a large amount of phosphogypsum, and the utilization rate of the phosphogypsum in the ingredients is above 80%.
[0025] Phosphogypsum can be used in large quantities to produce low-calcium clinker whose mineral composition is mainly low-calcium minerals C3S2 and CS, wherein the C3S2 content is 60-90%, the CS content is 10-30%, and the strength after carbonization is high.
[0026] Making the material into balls can reduce the contact between the carbonaceous raw materials in the balls and the air, making it easier to create a reducing atmosphere, thereby reducing the waste of carbonaceous raw materials.
[0027] On the premise that low KH value allows SiO2 to promote CaSO4 desulfurization to form a more stable and easier to generate mineral C2S, a lower KH value and total CaO:SiO2 are used to provide more SiO2 for desulfurization and lower the eutectic temperature, thereby solving the problem that the sphere is more difficult to burn and desulfurize than powder due to uneven heating and atmosphere conditions.
[0028] The raw materials used are all low-priced conventional raw materials in cement clinker production and can be obtained locally. After scientific formulation, the desulfurization effect of phosphogypsum is good and stable, the desulfurization rate reaches more than 99%, and the SO3 content in the calcined product is ≤1%. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : XRD pattern of the low-calcium clinker obtained in Example 1. DETAILED DESCRIPTION
[0030] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0031] A method for preparing low-calcium clinker by desulfurization of phosphogypsum is provided in a specific embodiment:
[0032] (1) obtaining phosphogypsum, carbonaceous raw materials, and silicon-aluminum-iron raw materials, drying, crushing, scientifically proportioning, and then mixing and grinding;
[0033] (2) adding water to the obtained mixture to form pellets, and then drying;
[0034] (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4;
[0035] (4) After the desulfurized material is cooled, it is added with siliceous raw materials for mixed grinding so that its KH value and the mass ratio of total CaO to SiO2 in the chemical composition meet the requirements of low-calcium clinker, and then enters the rotary kiln for calcination to obtain low-calcium clinker.
[0036] Specifically, the carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.
[0037] Specifically, the ferro-aluminum raw material in step (1) is one or more of sandstone, coal gangue, silica, clay, fly ash, and various types of waste residues.
[0038] Specifically, the scientific ingredients in step (1) are as follows: the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6.
[0039] Specifically, the diameter of the ball in step (2) is 1-3 cm.
[0040] Specifically, the desulfurization temperature of the desulfurization furnace in step (3) is 1150-1250°C.
[0041] Specifically, the siliceous raw material in step (4) is one or more of raw materials mainly containing SiO2, such as sandstone, coal gangue, silica, clay, fly ash, glass, and various waste residues.
[0042] Specifically, the KH value and the mass ratio of total CaO to SiO2 in the chemical composition in step (4) are 0.4-0.45 and 1.2-1.4 respectively.
[0043] Specifically, the calcination temperature of the rotary kiln in step (4) is 1200-1300°C.
[0044] Specifically, the mineral composition of the low-calcium clinker obtained in step (4) is mainly low-calcium minerals C3S2 and CS, wherein the content of C3S2 is 60-90%, and the content of CS is 10-30%.
[0045] The acquisition and detection of raw materials in the following specific examples:
[0046] Obtain phosphogypsum and silicon-aluminum-iron raw materials, and perform chemical composition analysis after drying, crushing and grinding. For example, the chemical composition of a batch of phosphogypsum and coal gangue obtained randomly is shown in Table 1:
[0047] Table 1 Chemical composition analysis
[0048] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43
[0049] The carbonaceous raw material used was subjected to conventional analysis and chemical composition analysis of the ash, which is high-sulfur coal. The results are shown in Table 2 and Table 3 respectively:
[0050] Table 2 Conventional analysis of high sulfur coal
[0051] name Moisture Ash Volatile Matter Fixed carbon content Total sulfur Qnet,ad Qnet,d High sulfur coal 1.42 23.48 10.25 64.85 2.99 25.25 26.33
[0052] Table 3 Chemical composition analysis of high sulfur coal ash
[0053] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40
[0054] Example 1
[0055] 1. Ratio design of phosphogypsum desulfurization
[0056] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss of 19.27% + 42.46% = 61.73%. The remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.475, the SM value is 6.629, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.491. The design ratio is that the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal is 86: 14: 6.88, and the weight of ash introduced by high-sulfur coal is 6.88 * 0.2348 = 1.62. The ratio and corresponding indicators are shown in Table 4 and Table 5 respectively:
[0057] Table 4 Proportions
[0058] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 14 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62
[0059] Table 5 Indicators corresponding to the ratio
[0060]
[0061] 2. Ball making
[0062] The phosphogypsum, coal gangue and high-sulfur coal measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.
[0063] 3. Desulfurization of phosphogypsum
[0064] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1200°C.
[0065] 4. Add siliceous raw materials and calcine to obtain low calcium clinker
[0066] Add siliceous raw materials to the desulfurized material for mixed grinding. The siliceous raw materials used here are coal gangue. The amount of coal gangue is equivalent to 14 in step 1 plus 2.5, so that the KH value and the mass ratio of total CaO to SiO2 in the chemical composition are 0.423 and 1.343 respectively. The proportion of low-calcium clinker and the corresponding indicators are shown in Table 6 and Table 7 respectively:
[0067] Table 6 Proportion
[0068] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 16.5 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62
[0069] Table 7 Indicators corresponding to the ratio
[0070]
[0071] Then it enters the rotary kiln for calcination to produce low-calcium clinker. The temperature of the rotary kiln is set at 1260℃.
[0072] 5. Carbonization of low calcium clinker
[0073] The obtained low-calcium clinker was ground into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 5 MPa and a water-solid ratio of 0.16. It was carbonized for 20 hours under the conditions of a carbon dioxide concentration of 100%, a temperature of 50°C, and an air pressure of 0.3 MPa, and then the compressive strength was measured.
[0074] Comparative Example 1
[0075] 1. Ratio design of phosphogypsum desulfurization
[0076] The SO3 in the chemical composition of phosphogypsum is calculated into its own ignition loss, and the remaining chemical composition is measured according to the ignition loss of 19.27% + 42.46% = 61.73%. The remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.666, the SM value is 6.157, and the mass ratio of total CaO to SiO2 in the chemical composition is 2.033. The design ratio is that the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal is 91.5: 8.5: 7.32, and the weight of ash introduced by high-sulfur coal is 7.32 * 0.2348 = 1.72. The ratio and corresponding indicators are shown in Table 8 and Table 9 respectively:
[0077] Table 8 Proportions
[0078] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 91.5 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 8.5 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.72
[0079] Table 9 Indicators corresponding to the ratio
[0080]
[0081] 2. Ball making
[0082] The phosphogypsum, coal gangue and high-sulfur coal measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.
[0083] 3. Desulfurization of phosphogypsum
[0084] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1200°C.
[0085] Comparative Example 2
[0086] 1. Ratio design of phosphogypsum desulfurization
[0087] Directly adopt the ratio of step 4 of Example 1 for desulfurization, calculate the SO3 in the chemical composition of phosphogypsum into its own ignition loss, according to the ignition loss 19.27% + 42.46% = 61.73%, the remaining chemical composition corresponds to the material mainly composed of CaO, and the molar ratio of C in the carbonaceous raw material to SO3 in the phosphogypsum is 0.8146, the KH value is 0.423, and the SM value is 6.771. , the total CaO and SiO2 mass ratio in the chemical composition is 1.343 for design ratio, that is, the amount of high-sulfur coal = the amount of phosphogypsum * 0.4246 * 0.8146 * 12 / (80 * 0.6485), the weight ratio of phosphogypsum: coal gangue: high-sulfur coal is 86: 16.5: 6.88, the weight of ash introduced by high-sulfur coal is 6.88 * 0.2348 = 1.62, the ratio and corresponding indicators are shown in Table 10 and Table 11 respectively:
[0088] Table 10 Proportions
[0089] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 16.5 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62
[0090] Table 11 Indicators corresponding to the ratio
[0091]
[0092] 2. Ball making
[0093] The phosphogypsum, coal gangue and high-sulfur coal measured in the above ratio are mixed and ground, and then water is added to form a ball with a diameter of 2 cm, and then naturally dried for 1 day.
[0094] 3. Desulfurization of phosphogypsum
[0095] The naturally dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4, and the temperature of the desulfurization furnace is set at 1200°C.
[0096] Comparative Example 3
[0097] Only steps 1, 2, and 3 in Example 1 are used. The desulfurized material obtained in step 3 is ground and made into a cylindrical sample with a diameter of 2 cm and a height of 2 cm at a molding pressure of 5 MPa and a water-solid ratio of 0.16. The sample is carbonized for 20 hours under the conditions of a carbon dioxide concentration of 100%, a temperature of 50°C, and an air pressure of 0.3 MPa, and then the compressive strength is measured.
[0098] Comparative Example 4
[0099] 1. Same as Example 1.
[0100] 2. Same as Example 1.
[0101] 3. Same as Example 1.
[0102] 4. Add siliceous raw materials and calcine to obtain low calcium clinker
[0103] Add siliceous raw materials to the desulfurized material for mixed grinding. The siliceous raw materials used here are coal gangue. The amount of coal gangue is equivalent to 14 in step 1 plus 6, so that the KH value and the mass ratio of total CaO to SiO2 in the chemical composition are 0.366 and 1.180 respectively. The proportion of low-calcium clinker and the corresponding indicators are shown in Table 12 and Table 13 respectively:
[0104] Table 12 Proportions
[0105] name Loss on ignition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[SO3]]> <![CDATA[K2O]]> <![CDATA[Na2O]]> Ratio Phosphogypsum 19.27 6.6 0.23 0.52 29.66 0.03 42.46 0.37 0.08 86 Coal Gangue 5.53 77.8 5.42 3.88 1.91 2.21 0.48 1.15 0.43 20 Coal ash 0 47.36 26.12 15.21 4.16 1.55 2.11 1.03 0.40 1.62
[0106] Table 13 Indicators corresponding to the ratio
[0107]
[0108] Then it enters the rotary kiln for calcination to produce low-calcium clinker. The temperature of the rotary kiln is set at 1260℃.
[0109] 5. Same as Example 1.
[0110] In addition to the temperature of 1150-1250°C described in the present invention, 1100°C was added to the desulfurization of phosphogypsum in each embodiment and comparative example. The content of SO3 in the desulfurized material is shown in Table 14, and the SO3 content is measured by total sulfur analysis. The content of main minerals in the desulfurized material is shown in Table 15, and the content of main minerals is obtained by analyzing the XRD spectrum of the calcined product (clinker) using jade software.
[0111] Table 14 SO3 content in desulfurized materials
[0112]
[0113] Table 15 Main mineral contents in desulfurized materials
[0114]
[0115]
[0116] According to the research of our institute, when the KH is 0.66, the total CaO:SiO2 is 2.0-2.3:
[0117] (1) Formation of aluminum-iron phase mineral C in the ingredients 12 The part of CaSO4 in A7, C3A, C4AF and C2F relies on Fe2O3 and Al2O3 for desulfurization. The desulfurization effect of Fe2O3 and Al2O3 on CaSO4 is worse than that of SiO2.
[0118] (2) Al2O3 combines with CaO and CaSO4 to form by-product minerals, which inhibit further desulfurization;
[0119] (3) C4AF and C2F are also difficult to burn in a reducing atmosphere and cannot be formed well, resulting in a decrease in the direct desulfurization effect of Fe2O3 on CaSO4 (the part of CaSO4 required to form iron-phase minerals) and the indirect desulfurization effect (fluxing to promote the formation of C2S);
[0120] (4) The desulfurization of CaSO4 has reached the limit chemical equilibrium that can be adjusted under the KH at this time, and the SO3 content is between 1% and 3%. After using conventional raw materials, the SO3 content in the calcined product is 2%.
[0121] The present invention, under the condition of a carbonaceous raw material providing a reducing atmosphere, is based on a low KH (KH value is 0.66) ingredient to make SiO2 promote the desulfurization of CaSO4 to form a more stable and easier to generate mineral C2S. The method continues to optimize and improve, reduces KH to a total CaO:SiO2 ratio of less than 2, provides more SiO2 for desulfurization, makes all CaSO4 have SiO2 and excess SiO2 is used to match, thereby generating calcium silicate-containing minerals, allows the desulfurization chemical equilibrium of SiO2 on CaSO4 to continue to move in the direction of desulfurization, and reduces the negative impact of Fe2O3 and Al2O3 that cannot further desulfurize CaSO4.
[0122] Compared with Example 1, Comparative Example 1 mainly has a higher KH value (higher total CaO:SiO2), that is, the company has made a breakthrough in the decomposition and desulfurization of phosphogypsum in recent research, and applied for an invention patent for "a phosphogypsum desulfurization and cement production process", which mainly adopts a method of mixing and desulfurization with low KH value ingredients, and the KH value is 0.6-0.7, so that SiO2 promotes CaSO4 desulfurization to form a more stable and easier to generate mineral C2S, but the content of SO3 after calcination at 1100°C is 1-3%, which cannot be reduced to less than 1%, and the desulfurization is carried out in powder form. Comparative Example 1 uses balling, which is more difficult to burn and desulfurize than powder due to uneven heating and atmosphere conditions, and when KH is 0.66, the high SM value will aggravate the difficulty in burning due to insufficient liquid phase minerals, so the SO3 content reaches 10.13% after calcination at 1100°C; the difficulty in burning is improved after the temperature reaches 1200°C, and the final SO3 content is 2-3%.
[0123] Example 1 Based on the premise that SiO2 promotes CaSO4 desulfurization at low KH value to form a more stable and easier to generate mineral C2S, a lower KH value and total CaO:SiO2 are used to provide more SiO2 for desulfurization and reduce the eutectic temperature, thereby solving the problem that the sphere is difficult to burn and desulfurize due to uneven heating and atmosphere conditions compared to powder at high SM value. The higher SM value reduces the negative impact of Fe2O3 and Al2O3 that cannot further desulfurize CaSO4, and successfully reduces the final SO3 content to less than 1%. A high desulfurization rate has been achieved at 1100℃, and desulfurization is based on the formation of C2S.
[0124] Compared with Example 1, Comparative Example 2 directly adopts the ratio of step 4 in Example 1 for desulfurization. Since the total CaO and SiO2 mass ratio is relatively low, which is 1.343, the melting point is lower, and a large amount of CaSO4 itself has a strong fluxing effect in the desulfurization process, resulting in severe melting of the sample, which is not conducive to production and also causes the desulfurization effect of CaSO4 to deteriorate. The SO3 content in the material after desulfurization is 1.24% (greater than 1%). Since part of the vitrified melt is amorphous, quantitative analysis of the jade mineral composition cannot be performed.
[0125] The main mineral contents in the prepared low-calcium clinker are shown in Table 16, and the carbonization conditions and strength of the low-calcium clinker after carbonization are shown in Table 17.
[0126] Table 16 Main mineral contents in the low calcium clinker produced
[0127] project Calcination temperature <![CDATA[C3S2]]> CS <![CDATA[C2S]]> <![CDATA[SiO2]]> <![CDATA[Ca2Al2SiO7]]> <![CDATA[CaSO4]]> <![CDATA[C4A3S-]]> Unknown sulfur-containing mineral Example 1 1260℃ 75.9 18.3 0 0.7 4.5 0 0 0 Comparative Example 3 / 70.6 0 17.3 1.5 10.0 0 0 0 Comparative Example 4 1260℃ 47.6 42.7 0 0.9 8.2 0 0 0
[0128] Table 17 Carbonization conditions and strength after carbonization of low calcium clinker
[0129]
[0130] The carbonization rate of CS mineral is lower than that of C3S2, and the carbonization strength is also lower than that of C3S2. However, too fast a carbonization rate will make the surface of the sample dense too early, and eventually CO2 cannot enter the interior of the sample, which reduces the degree of carbonization and thus the carbonization strength. Therefore, while C3S2 provides the main carbonization strength, an appropriate amount of CS with a slow carbonization rate should be introduced to increase the degree of carbonization. The CS content in the low-calcium clinker of C3S2 and CS should not be too high, otherwise the strength will be low, such as Comparative Example 4. Comparative Example 3 is the material after desulfurization. Since too high or too low a total CaO:SiO2 ratio in the desulfurization ingredients will cause the desulfurization effect of CaSO4 to deteriorate, it is impossible to adjust C3S2, CS, and C2S minerals to a better value to exert better carbonization strength. Figure 1 This is the XRD spectrum of the low-calcium clinker prepared in Example 1. The jade quantitative analysis results are C3S2=75.9%, CS=18.3%. It is a better low-calcium mineral ratio design with high strength after carbonization.
[0131] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A method for preparing low-calcium clinker by desulfurization of phosphogypsum, characterized in that The following steps are involved: (1) obtaining phosphogypsum, carbonaceous raw materials, and ferro-aluminum raw materials, drying, crushing, mixing and grinding the raw materials; the raw materials are prepared such that the molar ratio of C in the carbonaceous raw materials to SO3 in the phosphogypsum is 0.7-0.9, the KH value is 0.4-0.5, and the mass ratio of total CaO to SiO2 in the chemical composition is 1.4-1.6; (2) Add water to the obtained mixture to form pellets and dry them; (3) The dried pellets are placed in a desulfurization furnace for desulfurization with CaSO4; the desulfurization temperature of the desulfurization furnace is 1150-1250°C; (4) After the desulfurized material is cooled, it is added to the siliceous raw material and mixed and ground so that its KH value and the mass ratio of total CaO to SiO2 in the chemical composition meet the requirements of the designed low-calcium clinker, and then it is calcined in a rotary kiln to obtain low-calcium clinker; the KH value and the mass ratio of total CaO to SiO2 in the chemical composition are 0.4-0.45 and 1.2-1.4 respectively; the calcination temperature of the rotary kiln is 1200-1300°C.
2. The method for preparing low-calcium clinker by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The carbonaceous raw material in step (1) is one or more of ordinary coal, high-sulfur coal, and coke.
3. The method for preparing low-calcium clinker by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The ferro-aluminum-silicon raw material in step (1) is one or more of sandstone, coal gangue, silica, clay and fly ash.
4. The method for preparing low-calcium clinker by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The diameter of the ball in step (2) is 1-3 cm.
5. The method for preparing low-calcium clinker by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The siliceous raw material in step (4) is one or more of sandstone, coal gangue, silica, clay, fly ash and glass.
6. The method for preparing low-calcium clinker by desulfurization of phosphogypsum as claimed in claim 1, characterized in that The mineral composition of the low-calcium clinker obtained in step (4) is mainly low-calcium minerals C3S2 and CS, wherein the content of C3S2 is 60-90% and the content of CS is 10-30%.
Citation Information
Patent Citations
Process for co-production of cement by desulfurization of phosphogypsum
CN115073030A
Process for preparing calcium sulphoaluminate modified Portland cement clinker by phosphogypsum desulfurization
CN115180846A