A cement raw material admixture and preparation method thereof
By using raw meal admixtures such as butyl octanol residual liquid in cement production, the problems of low raw meal grinding efficiency and high energy consumption in cement production are solved, and the coal consumption of clinker burning and grinding power consumption are reduced. The effect is of significant economic and social value.
Patent Information
- Application Number
- CN202310350429.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-04
AI Technical Summary
In cement production, energy consumption and harmful gas emissions are large during the clinker preparation process. Existing cement admixtures are mainly used in the cement grinding stage and cannot be effectively used in the raw meal grinding stage, resulting in low efficiency.
A kind of cement raw meal additive is used, including butyl octanol residual liquid, modifier, performance regulator and dioctyl sulfosuccinate sodium salt, and is used as a raw meal additive after stirring evenly to improve the quality of raw meal powder. Grinding efficiency and reducing coal consumption for clinker burning.
It improves the efficiency of raw meal grinding and the coal consumption of clinker burning, realizes the reuse of resources, reduces the power consumption of grinding and the energy consumption of clinker burning, and has economic benefits and social value.
Smart Images

Figure BDA0004161309230000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement admixtures, and in particular relates to a cement raw material admixture and a preparation method thereof. Background Art
[0002] Cement is an important part of the national economy. According to statistics, the cement industry consumes a huge amount of standard coal every year, accounting for about 11% of the annual standard coal production. It is a major energy consumer, of which clinker production accounts for more than 90% of the total energy consumption of cement production. Our country is currently in urgent need of more advanced technologies to reduce energy consumption and harmful gas emissions in the clinker preparation process.
[0003] The cement production process can be summarized as "two grindings and one burning", namely raw material grinding, clinker burning, and cement grinding. The raw material grinding process is the key link in the production of new dry cement. The quality of raw material powder directly affects the subsequent raw material decomposition and clinker burning. Effective raw material grinding can greatly reduce the energy consumption of clinker burning.
[0004] At present, cement admixtures used in cement industry are mostly used in cement grinding stage, and rarely in raw material grinding stage. Most of the raw materials are ground by vertical mill grinding process, which has high grinding efficiency and short material residence time in the mill. Traditional cement admixtures have little effect on raw material grinding process. The research on admixtures used in raw material grinding stage is not systematic, and the application proportion of admixtures in raw material grinding stage is very small.
[0005] Butanol and n-octanol are mainly used to produce plasticizers dibutyl phthalate DBP and dioctyl phthalate DOP. With the rapid development of the petrochemical industry, the production of plastics is increasing rapidly, and the market demand for butanol and octanol (referred to as butanol and octanol) is also increasing year by year. In the device for producing butanol and octanol by carbonyl synthesis, due to process requirements, a large amount of waste liquid containing aldehydes, alcohols, acids, esters and their polymers and a small amount of phosphorus, catalysts, etc. is discharged, commonly known as butanol and octanol residue. Due to the complex composition of this part of the residue, it has not been reasonably recovered and utilized for a long time, and the economic benefits are poor. Summary of the invention
[0006] The purpose of the present invention is to provide a raw material admixture and a preparation method thereof. The raw material admixture provided by the present invention can utilize the residual liquid generated in the production process of butyl octanol, and has the comprehensive effects of improving the raw material grinding efficiency, reducing the grinding power consumption, and reducing the coal consumption of clinker burning.
[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0008] A cement raw material admixture is prepared from the following raw materials in parts by weight: 100-300 parts of butyl octanol residual liquid, 5-18 parts of a modifier, 3-6 parts of a performance regulator, and 0.1-0.5 parts of sodium salt of dioctyl sulfonate succinate.
[0009] Preferably, the butanol residue is a residue produced during the production of butanol using an oxo synthesis process.
[0010] The main components of the butanol-octanol residue mainly include alcohols such as butanol and octanol and aldehydes such as butyraldehyde and octenal. Alcohols such as butanol and octanol account for about 5-50% of the weight of the residue; aldehydes such as butyraldehyde and octenal account for about 5-40% of the weight of the residue.
[0011] Preferably, the modifier is one or more of citric acid, boric acid and hydrogen peroxide.
[0012] More preferably, the weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 1-10:1-5:3.
[0013] More preferably, the mass concentration of the hydrogen peroxide is 18-25%.
[0014] Preferably, the performance regulator is barium petroleum sulfonate or sodium trifluoromethane sulfonate.
[0015] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0016] (1) preparing various raw materials by weight, adding a modifier to the residual butyl octanol solution, stirring for 30-60 minutes, mixing evenly, and obtaining a mixed solution;
[0017] (2) adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, to obtain the raw material admixture.
[0018] The dosage of the admixture of the present invention is 0.15-0.3% of the raw material mass
[0019] After the raw material admixture butanol residual liquid of the present invention is added with a modifier and a regulator, the components are fully modified and optimized, and the macromolecular substances contained therein can stabilize the material layer when the vertical mill or the roller press is used to grind the raw material, improve the rolling efficiency, and do not affect the powder selection after drying, and the small molecule alcohols therein can improve the dispersibility of the material and improve the powder selection efficiency. Organic acid salts and sodium salts of dioctyl sulfosuccinate can wedge into the surface layer of the raw material, reduce the activation energy of calcium carbonate decomposition, and increase the decomposition rate of calcium carbonate; the elements such as fluorine, phosphorus, and rhodium contained therein can reduce the eutectic point of each mineral in the process of clinker formation, reduce the liquid phase formation temperature and viscosity, and promote clinker burning; and the butanol residual liquid contains a large amount of high molecular weight, high carbon content organic matter, has a high calorific value, and provides certain energy support for the decomposition of raw materials. In the present invention, various components are composed according to specific dosages, and the composite exerts a superposition effect, effectively improving the raw material grinding efficiency and reducing the coal consumption of clinker burning.
[0020] Beneficial Effects
[0021] The admixture of the present invention not only improves the raw material grinding efficiency and reduces the grinding power consumption, but also reduces the clinker standard coal consumption. It can also absorb the waste liquid from the chemical process and realize resource utilization, and has significant economic and social value and potential for actual market application. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.
[0023] Example 1
[0024] A cement raw material admixture is prepared from the following raw materials in parts by weight: 100 parts of butyl octanol residual liquid, 18 parts of a modifier, 3 parts of a performance regulator, and 0.5 parts of sodium salt of dioctyl sulfonate succinate.
[0025] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0026] The weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 10:1:3.
[0027] The mass concentration of the hydrogen peroxide is 25%.
[0028] The performance regulator is sodium trifluoromethanesulfonate.
[0029] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0030] (1) preparing various raw materials according to weight, adding a modifier to the residual liquid of butyl octanol, stirring for 30 minutes, mixing evenly, and obtaining a mixed liquid;
[0031] (2) adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, to obtain the raw material admixture.
[0032] Example 2
[0033] A cement raw material admixture is prepared from the following raw materials in parts by weight: 300 parts of butyl octanol residual liquid, 5 parts of a modifier, 6 parts of a performance regulator, and 0.1 parts of sodium salt of dioctyl sulfonate succinate.
[0034] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0035] The weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 1:5:3.
[0036] The mass concentration of the hydrogen peroxide is 18%.
[0037] The performance regulator is barium petroleum sulfonate.
[0038] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0039] (1) preparing various raw materials according to weight, adding a modifier to the residual liquid of butyl octanol, stirring for 60 minutes, mixing evenly, and obtaining a mixed liquid;
[0040] (2) adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, to obtain the raw material admixture.
[0041] Example 3
[0042] A cement raw material admixture is prepared from the following raw materials in parts by weight: 200 parts of butyl octanol residual liquid, 13 parts of a modifier, 5 parts of a performance regulator, and 0.3 parts of sodium salt of dioctyl sulfonate succinate.
[0043] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0044] The weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 8:2:3.
[0045] The mass concentration of the hydrogen peroxide is 22%.
[0046] The performance regulator is sodium trifluoromethanesulfonate.
[0047] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0048] (1) preparing various raw materials according to weight, adding a modifier to the residual liquid of butyl octanol, stirring for 50 minutes, mixing evenly, and obtaining a mixed liquid;
[0049] (2) adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, to obtain the raw material admixture.
[0050] Example 4
[0051] A cement raw material admixture is prepared from the following raw materials in parts by weight: 160 parts of butyl octanol residual liquid, 12 parts of a modifier, 4 parts of a performance regulator, and 0.3 parts of sodium salt of dioctyl sulfonate succinate.
[0052] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0053] The weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 7:4:3.
[0054] The mass concentration of the hydrogen peroxide is 25%.
[0055] Preferably, the performance modifier is sodium trifluoromethanesulfonate.
[0056] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0057] (1) preparing various raw materials according to weight, adding a modifier to the residual liquid of butyl octanol, stirring for 60 minutes, mixing evenly, and obtaining a mixed liquid;
[0058] (2) adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, to obtain the raw material admixture.
[0059] Comparative Example 1
[0060] A cement raw material admixture is prepared from the following raw materials in parts by weight: 200 parts of butanol residual liquid, 5 parts of a performance regulator, and 0.3 parts of sodium salt of dioctyl sulfonate succinate.
[0061] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0062] The performance regulator is sodium trifluoromethanesulfonate.
[0063] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0064] (1) Prepare various raw materials according to weight, add the performance regulator to the residual liquid of butyl octanol, stir evenly, and finally add sodium salt of dioctyl sulfonate succinate, mix evenly, and thus obtain the raw material admixture.
[0065] In this comparative example, except that no modifier is used, the remaining raw materials and process steps are the same as those of Example 3.
[0066] Comparative Example 2
[0067] A cement raw material admixture is prepared from the following raw materials in parts by weight: 200 parts of butyl octanol residual liquid, 13 parts of a modifier, and 0.3 parts of sodium salt of dioctyl sulfosuccinate.
[0068] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0069] The weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 8:2:3.
[0070] The mass concentration of the hydrogen peroxide is 22%.
[0071] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0072] (1) preparing various raw materials according to weight, adding a modifier to the residual liquid of butyl octanol, stirring for 50 minutes, mixing evenly, and obtaining a mixed liquid;
[0073] (2) Add sodium dioctyl sulfosuccinate to the mixed solution obtained in step (1), and mix well to obtain the raw material admixture.
[0074] In this comparative example, except that the performance regulator is not used, the other raw materials and process steps are the same as those of Example 3.
[0075] Comparative Example 3
[0076] A cement raw material admixture is prepared from the following raw materials in parts by weight: 200 parts of butyl octanol residual liquid and 0.3 parts of sodium salt of dioctyl sulfosuccinate.
[0077] The butanol residue is a residue produced during the production of butanol using a carbonyl synthesis process.
[0078] A method for preparing a cement raw material admixture comprises the following preparation steps:
[0079] (1) Prepare various raw materials by weight, add sodium salt of dioctyl sulfosuccinate to the residual liquid of butyl octanol, and mix well.
[0080] The raw material admixture is obtained.
[0081] In this comparative example, except that no modifier and performance regulator are used, the remaining raw materials and process steps are the same as those of Example 3.
[0082] Grinding aid effect test
[0083] The grinding aid performance of the admixtures in Examples 1-4 and Comparative Examples 1-3 of the present invention was tested according to the standard T / CCAS 021-2021 "Cement Raw Meal Grinding Aids". The limestone, aluminum, silicon, and iron materials were taken from Jining Conch Cement Co., Ltd. The experimental method is as follows:
[0084] (1) Sample preparation: All raw materials are pre-homogenized, crushed to 7 mm, and then re-homogenized. The raw materials after the second homogenization are placed in a drying oven at 105℃±5℃ for no less than 4 hours for use. One part is used to prepare a blank sample without raw material grinding aid, and the other part is used to prepare a comparison sample with raw material grinding aid.
[0085] (2) Preparation of blank sample: According to the mixing ratio, limestone 84% (4.2kg), clay 6% (0.3kg), iron tailings 6% (0.3kg), quartz sand 4% (0.2kg), prepare 5kg. Grind in a ball mill until the residue on the 80μm square mesh sieve is 16% to 18%, and record the grinding time Ts.
[0086] (3) Preparation of samples with raw material grinding aid: Mix the raw materials according to the specified raw material ratio, prepare 2 portions, each of which is 5 kg, and evenly add the raw material grinding aid according to the recommended dosage (internal addition) to the raw material. Grind for Ts time and grind twice. Discard the first grinding sample with raw material grinding aid and take the second grinding sample for testing.
[0087] (4) Sample testing: After grinding, the sample was passed through a 0.9 mm sieve to remove large particles, and the 80 μm sieve residue and the 200 μm sieve residue were measured.
[0088] Determination of the burnability of raw meal: The effect of admixtures on the burnability of raw meal was tested according to GB / T 26566-2011 "Test method for burnability of cement raw meal", and the test temperature was 1350℃ and 1400℃.
[0089] The test results are shown in Table 1 below.
[0090] Table 1 Performance test results
[0091]
[0092] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A cement raw material admixture, characterized in that: The invention is prepared from the following raw materials in parts by weight: 100-300 parts of butyl octanol residual liquid, 5-18 parts of a modifier, 3-6 parts of a performance regulator, and 0.1-0.5 parts of sodium salt of dioctyl sulfonated succinate; the butyl octanol residual liquid is a residual liquid produced in the process of producing butyl octanol by a carbonyl synthesis process; the weight ratio of citric acid, boric acid and hydrogen peroxide in the modifier is 1-10:1-5:3; and the performance regulator is petroleum barium sulfonate or sodium trifluoromethanesulfonate.
2. The cement raw material admixture according to claim 1, characterized in that: The mass concentration of the hydrogen peroxide is 18-25%.
3. A method for preparing the cement raw material admixture according to any one of claims 1 to 2, characterized in that: The method comprises the following preparation steps: (1) Prepare the raw materials according to weight, add the modifier to the residual liquid of butyl octanol, stir for 30-60 minutes, mix evenly, and obtain a mixed liquid; (2) Adding a performance regulator to the mixed solution obtained in step (1), stirring evenly, and finally adding sodium salt of dioctyl sulfonate succinate, mixing evenly, thereby obtaining the raw material admixture.
Citation Information
Patent Citations
Pretreatment method for co-processing of organic waste liquid in cement kiln
CN103453533A
Alcohol-hydrocarbon composite fuel for boiler and preparation method of alcohol-hydrocarbon composite fuel
CN106497614A