An organic Janus nanosheet-stabilized water-based carbon dioxide foam and its preparation method and application
By forming a dense nano-armor layer of organic Janus nanosheets on the surface of CO2 foam, the problem of poor stability of CO2 foam is solved, the storage efficiency and amount of CO2 are improved, and efficient CO2 storage is achieved.
Patent Information
- Application Number
- CN202310017710.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-06
AI Technical Summary
Existing technology is difficult to effectively stabilize CO2 foam, resulting in gravity differentiation and fingering of CO2 during formation flow, which reduces storage efficiency and quantity. In particular, two-dimensional nanoparticles have poor stability at the air-water interface and are difficult to inhibit CO2 diffusion. .
Organic Janus nanosheets are used to form a dense nano-armor layer through the uniform distribution of hydrophobic and hydrophilic groups, inhibiting the diffusion of CO2, and improving the stability and fluidity control capabilities of the foam by controlling the size and morphology of the nanosheets.
It achieves the preparation of ultra-stable water-based CO2 foam under low-cost and mild conditions, enhances the storage safety and geological storage capacity of CO2, effectively inhibits CO2 channeling, and expands the scope of CO2 storage.
Smart Images

Figure HDA0004041155130000011 
Figure HDA0004041155130000012 
Figure HDA0004041155130000021
Abstract
Description
Technical Field
[0001] The invention relates to an organic Janus nanosheet-stabilized water-based carbon dioxide foam and a preparation method and application thereof, belonging to the technical fields of nanomaterial preparation technology and carbon sequestration and utilization. Background Art
[0002] Fossil fuels are one of the main sources of energy supply in the world. However, with the continuous growth of social demand, the massive consumption of fossil fuels has aggravated the emission of greenhouse gases such as CO2. Excessive emission of CO2 in the atmosphere has led to rising global temperatures and drastic climate changes. How to reduce the concentration of CO2 in the atmosphere has received widespread attention and attention from all over the world. Carbon capture, utilization and storage (CCUS) technology is considered to be one of the most effective solutions to reduce the concentration of CO2 in the atmosphere. Injecting CO2 into formations is currently one of the most promising methods for large-scale CO2 storage, such as injection into deep saline formations, abandoned oil and gas reservoirs, coal seams, and for oil and gas enhanced recovery. However, since CO2 has much lower viscosity and density than oil and water, and has high mobility, gravity differentiation and fingering are very likely to occur during the formation flow process, resulting in low sweep efficiency and storage capacity.
[0003] Foam is a multiphase fluid with high viscosity. It produces the Jamin effect during the flow of porous media, increasing the flow resistance and reducing the gas fluidity. Therefore, it is regarded as an efficient system for controlling fluidity. However, foam is a thermodynamically unstable system. Behaviors such as liquid separation, aggregation, and rupture weaken the foam effect. Based on the Pickering theory, the stability of the foam can be improved by adsorbing nanoparticles on the foam surface. A large number of studies have shown that the nanoparticle-surfactant system can prepare homogeneous foams with higher viscosity and has stronger fluidity control ability than foams prepared from pure surfactant solutions. Nanoparticle-enhanced foams can control the flow direction of the fluid and improve the sweep coefficient due to high Jamin resistance and wall friction resistance.
[0004] According to particle size and aspect ratio, nanoparticles can be mainly divided into three categories: zero-dimensional nanoparticles, one-dimensional nanoparticles (such as nanowires), and two-dimensional nanoparticles (such as nanosheets). Zero-dimensional nanoparticles are mainly spherical, and the commonly used material substrates are oxides of elements such as Si, Ti, Fe, and Al. The foam stabilization mechanism is mainly through adsorption at the gas-liquid interface and Plateau boundary of the foam, reducing the contact area between bubbles, forming a dense particle film to inhibit the aggregation and disproportionation of bubbles, prolong the drainage time of the liquid film, and improve the strength of the liquid film skeleton. In addition, nanoparticles can improve the viscoelasticity of the liquid film interface, and the self-recovery ability of the liquid film is enhanced when it is impacted by external forces. However, due to the morphological characteristics of zero-dimensional nanomaterials, they are partially stacked and adsorbed on the surface of the liquid film, which is prone to slippage, resulting in the limitation of the effect of slowing down the aggregation. In addition, compared with air or nitrogen, CO2 has stronger diffusivity and worse stability of CO2 foam. Spherical zero-dimensional nanomaterials have a small aspect ratio and size, and the amount required to form a nano-enhanced film when adsorbed at the gas-liquid interface is larger, and the gaps between the particles are large, which limits the inhibitory effect on CO2 diffusion. One-dimensional nanoparticles mainly improve the stability of the foam by forming a network structure in the liquid film to increase the viscosity of the liquid phase, thereby inhibiting the thinning of the liquid film caused by the liquid film. On the other hand, one-dimensional nanoparticles can promote the closer arrangement of surfactant molecules at the interface, increase the difficulty of gas permeation through the liquid film, and thus slow down the aggregation and disproportionation of bubbles. However, the disadvantages of one-dimensional nanoparticles are also obvious. The mechanical strength of the liquid film cannot be effectively enhanced, and the distribution of one-dimensional nanoparticles on the surface of the liquid film is generally uneven. At slightly higher concentrations, they are prone to entanglement and aggregation into macromolecular polymers, making it difficult for them to maintain a stable state at the phase interface. In addition, similar to zero-dimensional nanoparticles, one-dimensional nanoparticles still require a large number of particles to be adsorbed when stabilizing CO2 foam, resulting in increased costs.
[0005] Based on the above problems, two-dimensional nanoparticles have attracted attention for stabilizing the phase interface. First, from the morphological analysis, compared with zero-dimensional and one-dimensional nanoparticles, two-dimensional nanoparticles have the potential to be more stably adsorbed on the phase interface due to their unique sheet morphology and larger aspect ratio, thus forming an interface armor film at the interface, which is not easy to fall off, has a small amount of use, and the gaps between nanosheets are small, and the mass transfer phenomenon between bubbles is limited, so it has a stronger potential to inhibit the diffusion of CO2 between bubbles. Secondly, according to the adsorption energy, it can be seen that it is difficult for two-dimensional nanosheets to effectively adsorb to the surface of emulsions or bubbles to improve stability, which is mainly affected by the hydrophilic and hydrophobic properties of nanosheets and size control. Thanks to the two-sided characteristics of nanosheets, inspired by the molecular structure of surfactants, the two sides of the two-dimensional nanosheets can be given hydrophilic and hydrophobic properties respectively, so that they obtain opposite properties, namely Janus properties, so that Janus particles spontaneously tend to the phase interface to form a stable reinforcement layer of emulsions or foams. At present, two-dimensional Janus nanosheets are often used to prepare Pickering emulsions, which have great application value in cosmetics, construction, medicine and other industries. However, compared with the oil-water interface, the interfacial tension of the foam gas-water interface is greater, and gas diffusion and other phenomena are more intense, especially CO2 gas. Therefore, the stability of the gas-water interface is more difficult, and there are few reports on Janus nanosheets stabilizing foam. The strong instability of foam poses a great challenge to the hydrophilic-hydrophobic balance and the size of Janus nanosheets that are easy to adsorb tightly. Therefore, it is necessary to provide a method that can achieve low-cost and mild conditions to synthesize Janus nanosheets, and can be used to tightly coat the foam surface to form an ultra-stable water-based CO2 foam, so as to effectively control the mobility of CO2 in the process of migration in porous media and improve the safety and geological storage of CO2. Summary of the invention
[0006] The purpose of the present invention is to provide an organic Janus nanosheet-stabilized water-based carbon dioxide foam, wherein the amphiphilic groups of the two-dimensional organic Janus nanosheet are evenly distributed, the Janus characteristics are strong, the size of the nanosheet is controllable, and the synthesis is simple; the two-dimensional organic Janus nanosheet involved in the present invention can form a dense nano armor layer on the surface of the bubble, inhibit CO2 diffusion, and improve the foam stability; the nano armor layer has strong interface viscoelasticity, can effectively inhibit CO2 cross-flow, control CO2 mobility, and help expand the CO2 storage range and increase the geological storage capacity.
[0007] The “two-dimensional nanomaterial” mentioned in the present invention refers to a nanomaterial with one dimension in nanometer size, such as nanosheets, nanofilms, etc.
[0008] The present invention first provides a method for preparing an organic Janus nanosheet, comprising the following steps:
[0009] S1. Grind the hydrophobic end molecules containing long-chain alkanes and primary amino groups thoroughly in a mixture of ethanol or other monohydric alcohols and water, and stir slowly at a temperature 3 to 5°C higher than room temperature until the solution is free of turbidity and the hydrophobic end molecules are completely dissolved. During this period, avoid large-scale shaking to allow them to arrange themselves in an orderly manner;
[0010] S2, adding a hydrophilic end molecule containing a hydroxyl group and a hydrophilic group to the solution of step S1, adding a small amount of weak acid and adjusting the pH value to 6.0-6.5, and gradually reducing the temperature by 5-10° C. every 20-30 minutes under an inert atmosphere to room temperature to synthesize an organic Janus nanosheet monomer, during which the color is observed to be significantly deepened, indicating that a nucleophilic addition reaction has occurred;
[0011] S3, adding ethanol to the solution of step S2 to adjust the solvent composition ratio, and dropping a weak acid to adjust the pH value to 6.0-6.5, and standing to react for 5-10 minutes; then adjusting the pH value to 7.0-8.0, adding sodium ethoxide, adjusting the temperature to 70-85° C., adding a condensing reflux device to react under an inert atmosphere, adding NaOH to the system to adjust the pH to 8.0-9.0, stirring until completely dissolved, stopping stirring and standing, and the organic Janus nanosheets can be obtained.
[0012] In the above preparation method, the hydrophobic end molecule is a long-chain alkane containing a primary amine group such as octadecylamine or dodecylamine;
[0013] The hydrophilic end molecule is an aromatic hydrocarbon compound containing a phenolic hydroxyl group and a hydrophilic group, such as dopamine, tyramine or 2,4-dihydroxyphenylethylamine.
[0014] In the above preparation method, in step S1, the mass ratio of the hydrophobic end molecule, the ethanol and the water is 1:20-100:10-50.
[0015] In the above-mentioned preparation method, in step S1, the step of spontaneous orderly arrangement is as follows:
[0016] The hydrophobic end molecules are added to the ethanol or other monohydric alcohol solution, and refluxed at 60-80° C. until dissolved; then the water is added, and stirring is stopped after no turbidity; and the spontaneous orderly arrangement is carried out at 50-70° C.
[0017] In the above preparation method, in step S2, the reflux conditions are as follows:
[0018] The initial temperature is 50-80°C, and it is lowered by 5-10°C every 20-30 minutes until it reaches room temperature.
[0019] In the system of step S2, the mass percentage of the hydrophilic end molecules is 0.5-1.5%;
[0020] The mass ratio of the hydrophilic end molecules to the hydrophobic end molecules is 1:2-5, preferably 1:3.
[0021] In the above preparation method, in step S3, the reaction time is 4 to 8 hours;
[0022] The mass ratio of the ethanol to the solution obtained in step S2 is 1:1.5-3;
[0023] In the system of step S3, the mass percentage of the sodium ethoxide is 0.1-0.4%.
[0024] In the above preparation method, in step S3, after the reaction is completed, the following purification step is also included:
[0025] Ethanol and water are sequentially added to the system of step S3 for ultrasonic dispersion and centrifugal treatment to obtain a solid product; the organic Janus nanosheets are stored in powder form after vacuum freeze drying; the thickness of the obtained Janus nanosheets is controlled to be 5 to 40 nm.
[0026] The above ultrasonic dispersion step can be carried out in small amounts and in multiple portions;
[0027] The ultrasonic dispersion time of the ethanol is 20 to 60 minutes;
[0028] The ultrasonic dispersion time of the water is 20 to 60 minutes;
[0029] The above ultrasonic dispersion step can be repeated 2 to 5 times.
[0030] In step S3, the volume ratio of the solution obtained, the ethanol and the water is 1:4-10:8-20.
[0031] The two-dimensional organic Janus nanosheet prepared by the method of the present invention has hydrophobic end groups and hydrophilic end groups synthesized in proportion to form the nanosheet, with more uniform group distribution and stronger Janus characteristics; the aspect ratio of the Janus nanosheet can be controlled and the shape is regular.
[0032] The contact angle test of the two-dimensional organic Janus nanosheet prepared by the method of the present invention shows that the two-dimensional organic Janus nanosheet has the ability of wettability reversal.
[0033] Based on the two-dimensional organic Janus nanosheets, the present invention further provides a stable water-based CO2 foam made of CO2 and a liquid phase;
[0034] The liquid phase is an aqueous solution of a surfactant and the organic Janus nanosheets;
[0035] The foam mass of the water-based CO2 foam is 40% to 95%, and more preferably 60% to 90%.
[0036] Specifically, in the liquid phase, the mass percentage of the surfactant is less than 1.0%, preferably 0.2% to 1.0%;
[0037] The mass percentage of the organic Janus nanosheets is less than 0.7%, preferably 0.05% to 0.7%, more preferably 0.05%, 0.08%, 0.1%, 0.15%, 0.18%, 0.2%, 0.3%, 0.4% or a range consisting of any two of the above values;
[0038] The surfactant may be an anionic surfactant, a cationic surfactant or a nonionic surfactant. The anionic surfactant is preferably sodium dodecyl sulfate (SDS), the cationic surfactant is preferably hexadecyltrimethylammonium bromide (CTAB), and the nonionic surfactant is preferably octylphenyl polyoxyethylene ether (TX-100).
[0039] The method for preparing the water-based CO2 foam of the present invention comprises the following steps:
[0040] Sa, adding the organic Janus nanosheets to the aqueous solution of the surfactant, stirring for 10 to 20 minutes to obtain a foam base liquid;
[0041] Sb, injecting CO2 into the foam base liquid, stirring and foaming by a Waring Blender method, to obtain the water-based CO2 foam;
[0042] The stirring speed can be 7000-9000 rpm, and the stirring time can be 3-10 min.
[0043] The organic Janus nanosheet ultra-stable water-based CO2 foam prepared by the method of the present invention was subjected to foaming and foam stabilization experiments. The results showed that the composite foam of non-ionic surfactant and organic Janus nanosheet has the strongest stability, and the foam stability becomes stronger with the increase of nanosheet concentration.
[0044] The present invention has the following beneficial effects:
[0045] (1) In the ultra-stable water-based CO2 foam system of the present invention, the two-dimensional organic Janus nanosheets can form a dense nano-armor layer on the surface of the bubble to inhibit the diffusion of CO2. Due to the large aspect ratio of the sheet, an efficient coating can be formed on the surface of the bubble. The organic Janus nanosheets can form a dense nano-armor layer at a low concentration to stabilize the CO2 foam, which helps to efficiently carry and seal CO2 in underground reservoirs.
[0046] (2) The ultra-stable water-based CO2 foam system of the present invention has a strong viscoelasticity of the interface of the nano-armor layer and a large flow resistance in the porous medium. Therefore, it can effectively block the crossflow channel and inhibit the CO2 fingering, thereby controlling the CO2 fluidity, expanding the CO2 storage range, and increasing the storage capacity.
[0047] (3) In the ultra-stable water-based CO2 foam system of the present invention, the Janus nanosheets have an electron-donating group (carbonyl group), i.e., a Lewis base compound, due to the structural characteristics of the hydrophilic / hydrophobic groups in the synthesis and preparation, which makes them more compatible with CO2 molecules and has a good CO2 gas encapsulation effect, thus helping to achieve the purpose of carbon capture, utilization and storage.
[0048] (4) In the ultra-stable water-based CO2 foam system of the present invention, the hydrophilic / hydrophobic groups do not participate in the reaction during the synthesis of the two-dimensional organic Janus nanosheets, and can therefore be replaced by other similar groups to flexibly change the hydrophilic and hydrophobic groups of the Janus nanosheets, and the reactants react in proportion to ensure that the hydrophobic end groups and the hydrophilic end groups are formed into sheets in a fixed ratio, so that the distribution of the amphiphilic groups is more uniform, and the prepared nanosheets have more significant Janus properties.
[0049] (5) In the ultra-stable water-based CO2 foam system of the present invention, the synthesis of two-dimensional organic Janus nanosheets does not require the construction of a phase interface, the preparation method is simple, the reaction conditions are mild, the synthesis process is short, the yield of Janus nanosheets is high, and the aspect ratio of the nanosheets can be controlled by adjusting the solution pH value and the synthesis time during the process to obtain Janus nanosheets in the target size range. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a SEM image of the organic Janus nanosheet prepared in Example 1 of the present invention.
[0051] Figure 2 The contact angles of the organic Janus nanosheets prepared in Example 1 of the present invention before and after wetting modification on the hydrophilic surface and the hydrophobic surface.
[0052] Figure 3 This is a particle size intensity diagram of Janus nanosheets prepared at different pH values and different reaction times in Example 2 of the present invention.
[0053] Figure 4 The foaming volume and liquid separation half-life of the foam formed by compounding the organic Janus nanosheets prepared in Example 3 of the present invention with a non-ionic surfactant vary with the concentration of the Janus nanosheets. DETAILED DESCRIPTION
[0054] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0055] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0056] Example 1. Synthesis of organic Janus nanosheets
[0057] (1) Hydrophobic end molecules spontaneously arrange in an orderly manner
[0058] Grind 1.2 g of octadecylamine (ODA) thoroughly and add it to 40 g of ethanol solution. Stir and reflux in a 75°C constant temperature water bath until the octadecylamine is completely dissolved. Slowly add 20 g of deionized water to the solution. Stop stirring when the solution is no longer turbid, so that the octadecylamine molecules are spontaneously arranged in an orderly manner in the ethanol-water system. Adjust the water bath temperature to 60-65°C.
[0059] (2) Synthesis of organic Janus nanosheet monomers
[0060] 0.4 g of dopamine (DA) was added to the solution in (1), and acetic acid was added to adjust the pH to 6.0-6.5. The mixture was refluxed under nitrogen atmosphere. The initial temperature was set to 60°C and then decreased by 5°C every 20 minutes. After 2 h of reaction, the heating was stopped and the solution was naturally cooled to room temperature to complete the synthesis of the organic Janus nanosheet monomer.
[0061] (3) Synthesis of organic Janus nanosheets
[0062] Add 40 g of ethanol to the solution in (2), and add acetic acid to adjust the pH to 6.0-6.5. Heat the solution in a water bath and condense under reflux for 7 minutes. Add ammonia water to adjust the pH of the solution to 7.5. Add 0.2 g of sodium ethoxide and adjust the temperature to 85°C. After stirring at a constant temperature for 6 hours under a nitrogen environment, add NaOH to adjust the pH to 8.0-9.0. Stop stirring after sufficient mixing and dissolution. Cool to room temperature and take out. The thickness is 20-30 nm.
[0063] (4) Purification of organic Janus nanosheets
[0064] Each time, 20 mL of the solution in (3) is taken, and after being fully mixed with 100 mL of ethanol solution, ultrasonic dispersion and centrifugation are performed for 20 minutes, the supernatant is removed, and the solid product is retained. 200 mL of deionized water is added to the separated product, ultrasonic dispersion and centrifugation are performed for 20 minutes, and the supernatant is removed, and the solid product is retained. The above two steps are repeated 2 to 3 times to obtain organic Janus nanosheets. The product is subjected to vacuum freeze drying to obtain powdered organic Janus nanosheets for storage.
[0065] Figure 1 This is a SEM image of the organic Janus nanosheet obtained in this example. It can be seen that the organic Janus nanosheet prepared in the present invention has a two-dimensional sheet structure.
[0066] Figure 2 The contact angles of the organic Janus nanosheets prepared in this example before and after wetting modification on the hydrophilic surface and the hydrophobic surface prove that the nanosheet material synthesized by the present invention has amphiphilic properties:
[0067] The glass substrate has hydrophilic properties, with a water contact angle of 57.6°. After the surface is hydrophobic, the contact angle becomes 136.1°. After the two substrates are coated with nanosheets, the wettability reversal phenomenon occurs, and the original hydrophilic / hydrophobic surface is transformed into a hydrophobic / hydrophilic surface. Therefore, according to the contact angle results, it can be confirmed that the nanosheet has amphiphilic properties.
[0068] Example 2: Controllable preparation of organic Janus nanosheets with different particle sizes
[0069] The operation steps are the same as those in Example 1, except that the pH value of the ammonia solution in the synthesis of organic Janus nanosheets in step (3) is changed, and the total reaction time of steps (2) and (3) is changed to test the effects of different pH values and different reaction times on the particle size of Janus nanosheets.
[0070] Figure 3 The particle size intensity diagram of the nanosheets prepared under different pH values and different reaction times shows that the particle size of the Janus nanosheets decreases with the increase of pH value and the shortening of reaction time. The size of the generated Janus nanosheets can be controlled by controlling different reaction times and pH values.
[0071] Example 3: Preparation of ultra-stable water-based CO2 foam using organic Janus nanosheets
[0072] A 0.4% by weight TX-100 surfactant solution was prepared, stirred for 5 minutes, and then the organic Janus nanosheets prepared in Example 1 were dissolved in the surfactant solution, and stirred for 20 minutes to obtain a foam base liquid compounded with Janus nanosheets and surfactants;
[0073] Pour the foam base liquid into a stirring cup, seal the stirring cup, introduce CO2 to form a CO2 environment in the cup, and use a Waring Blender method to stir and foam the foam base liquid at a stirring speed of 8000 rpm for 3 minutes to obtain CO2 foam, and the foam quality can be controlled to be 40% to 95%, and further controlled to be 60% to 90%.
[0074] Figure 4 The foaming effect of the compound of 0.4% by mass nonionic surfactant and different mass percentages of Janus nanosheets can be seen:
[0075] As the mass percentage of Janus nanosheets gradually increases to 0.15%, the nanosheet material in the solution is continuously adsorbed onto the bubble surface, gradually forming an armor-like coating state using its Janus properties and flaky morphology to prevent bubble drainage and aggregation, thereby achieving the effect of improving foam stability.
[0076] When the concentration of Janus nanosheets increases further, due to the limited interfacial area on the bubble surface, the nanosheet materials continue to aggregate and stack until the larger bubbles cannot withstand the adsorption of a large number of nanosheets and break, and the nanosheets return to the liquid phase, causing the solution viscosity to increase sharply. However, the increase in solution viscosity greatly reduces the liquid separation rate of smaller bubbles in the system. Therefore, the foaming volume of the foam system decreases at this stage, and the liquid separation half-life gradually increases.
Claims
1. A method for preparing an organic Janus nanosheet, comprising the following steps: S1, spontaneously arranging the hydrophobic end molecules in a mixture of ethanol and water; The hydrophobic end molecule is octadecylamine or dodecylamine; The mass ratio of the hydrophobic end molecule, the ethanol and the water is 1:20-100:10-50; S2, adding the hydrophilic end molecule to the solution of step S1, adjusting the pH value to 6.0-6.5, refluxing under an inert atmosphere, and synthesizing the organic Janus nanosheet monomer; The hydrophilic end molecule is dopamine, tyramine or 2,4-dihydroxyphenylethylamine; The reflux conditions are as follows: The initial temperature is 50~80℃, and it is lowered by 5~10℃ every 20~30 minutes until it reaches room temperature. In the system of step S2, the mass percentage of the hydrophilic end molecules is 0.5-1.5%; The mass ratio of the hydrophilic end molecule to the hydrophobic end molecule is 1:2-5; S3, adding ethanol to the solution of step S2, and adjusting the pH value to 6.0-6.5, heating and reflux; then adjusting the pH value to 7.0-8.0, adding sodium ethoxide, adjusting the temperature to 70-85° C., reacting under an inert atmosphere, adding NaOH to adjust the pH to 8.0-9.0, stirring until completely dissolved, to obtain the organic Janus nanosheet; The reaction time is 4 to 8 hours; The mass ratio of the ethanol to the solution obtained in step S2 is 1:1.5-3; The mass percentage of the sodium ethoxide is 0.1-0.4%; After the reaction is completed, the following purification step is also included: Adding ethanol and water to the system of step S3 in sequence, performing ultrasonic dispersion and centrifugation to obtain a solid product; In step S3, the volume ratio of the solution obtained, the ethanol and the water is 1:4-10:8-20.
2. The preparation method according to claim 1, characterized in that: In step S1, the steps of spontaneous orderly arrangement are as follows: The hydrophobic end molecules are added to the ethanol and refluxed at 60-80° C. until dissolved; then the water is added and stirring is stopped after no turbidity; and the spontaneous orderly arrangement is carried out at 50-70° C.
3. Organic Janus nanosheets prepared by the method of claim 1 or 2; The thickness of the Janus nanosheet is 5-40 nm.
4. Application of the organic Janus nanosheets according to claim 3 in carbon utilization and storage; The organic Janus nanosheets are used to form water-based CO2 foam.
5. An organic Janus nanosheet ultra-stable water-based CO2 foam made of CO2 and liquid phase; The liquid phase is an aqueous solution of a surfactant and the organic Janus nanosheets according to claim 3; The foam quality of the water-based CO2 foam is 40% to 95%.
6. The water-based CO2 foam according to claim 5, characterized in that: In the liquid phase, the mass percentage of the surfactant is less than 1.0%; The amount percentage of the organic Janus nanosheets is less than 0.7%; The surfactant is an anionic surfactant, a cationic surfactant or a nonionic surfactant.
7. The method for preparing the water-based CO2 foam according to claim 5 or 6, comprising the following steps: Sa, adding the organic Janus nanosheets into the aqueous solution of the surfactant, stirring to obtain a foam base liquid; Sb. Inject CO2 into the foam base liquid, and use a Waring Blender method to stir and foam to obtain the water-based CO2 foam.
8. Use of the water-based CO2 foam according to claim 5 or 6 in CO2 geological storage and foam oil recovery.