A glass fiber reinforced PBT-POK composition and its preparation method and application

Glass fiber reinforced PBT-POK compositions were prepared by compounding PBT-POK and adding glass fibers, compatibilizers, and calcium sulfate whiskers, which solved the shortcomings of POK resin in terms of thermal stability and wear resistance, and achieved an overall improvement in the material's performance.

CN116376262BActive Publication Date: 2024-11-19KINGFA SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310404224.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-11-19
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

POK resin is deficient in terms of thermal stability and wear resistance, making it difficult to meet market demands.

Method used

A glass fiber reinforced PBT-POK composition was prepared by compounding PBT resin with POK resin and adding glass fiber, compatibilizer, calcium sulfate whiskers and additives. The glass fiber improves the rigidity of the material, the compatibilizer enhances the molecular chain bonding, the calcium sulfate whiskers improve wear resistance, and the additives enhance the material performance.

Benefits of technology

It significantly improves the thermal stability and wear resistance of the material, reduces warpage, and enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004180708120000011
    Figure BDA0004180708120000011
  • Figure BDA0004180708120000061
    Figure BDA0004180708120000061
  • Figure BDA0004180708120000062
    Figure BDA0004180708120000062
Patent Text Reader

Abstract

The present invention discloses a glass fiber reinforced PBT-POK composition and a preparation method and application thereof. The glass fiber reinforced PBT-POK composition comprises the following components by weight: 100 parts of PBT resin; 60-120 parts of POK resin; 3-8 parts of compatibilizer; 40-60 parts of glass fiber; and 10-20 parts of calcium sulfate whisker. The glass fiber reinforced PBT-POK composition provided by the present invention has not only good thermal stability, but also good wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering plastics, and in particular to a glass fiber reinforced PBT-POK composition and a preparation method and application thereof. Background Art

[0002] As an engineering plastic, POK has excellent wear resistance, but it has problems such as poor thermal stability, easy carbonization, and serious degradation of thermal oxidative aging performance, which greatly limits the application of POK. With the development of technology, more and more products require materials with good thermal stability and wear resistance. However, the current performance of POK cannot meet the market demand for POK's thermal stability and wear resistance. Summary of the invention

[0003] In order to overcome the above-mentioned defects of the prior art, the present invention proposes a glass fiber reinforced PBT-POK composition and its preparation method and application. The specific technical scheme is as follows:

[0004] A glass fiber reinforced PBT-POK composition, comprising the following components in parts by weight:

[0005]

[0006] Due to the characteristics of the molecular structure of POK resin, the unstable end groups on the molecular chain will degrade under the action of heat and oxygen, resulting in a sharp drop in the thermal stability of the material. The addition of PBT resin will combine with some unstable end groups on the POK resin, thereby reducing the degree of degradation of the end groups due to heat and oxygen attack. The impact strength of PBT / POK material is not high. By adding a specific amount of glass fiber, the rigidity of PBT / POK material can be improved, so that the glass fiber reinforced PBT-POK composite has excellent tensile strength and notched impact strength.

[0007] Furthermore, the compatibilizer is ethylene-acrylic acid-glycidyl methacrylate. PBT and POK are only partially well combined, and ethylene-acrylic acid-glycidyl methacrylate is used as a compatibilizer, one end of which can be connected to PBT and the other end to POK, thereby further improving the combination between the PBT and POK molecular chains, achieving the effect of improving thermal stability and wear resistance.

[0008] Further, the melt index of the POK resin is 6-200 g / 10min, preferably 10-150 g / 10min, more preferably 20-120 g / 10min, and more preferably 30-100 g / 10min. The test standard of the melt index is ISO1133-1-2012, and the test conditions are 240°C and 2.16KG.

[0009] Furthermore, according to method A in GB / T 14190-2017, i.e., the capillary viscometer method, the intrinsic viscosity of the PBT resin is tested, the solvent used is phenol and 1,1,2,2-tetrachloroethane in a mass ratio of 50:50, and the intrinsic viscosity of the PBT resin at 25±0.05° C. is 0.72-1.2 dL / g. PBT / POK within this intrinsic viscosity range can achieve better mixing effects and balance fluidity and mechanical properties.

[0010] Furthermore, the width of the calcium sulfate whisker is 5-15 μm, and the thickness of the calcium sulfate whisker is 0.2-0.8 μm. The calcium sulfate whisker plays a role in improving wear resistance. In addition, under the condition of equal filler content, the calcium sulfate whisker replaces part of the glass fiber, which improves the wear resistance, improves the surface floating fiber effect of the material, improves the glossiness, and reduces the warpage. The length of the calcium sulfate whisker can be 50-200 μm.

[0011] Furthermore, the glass fiber reinforced PBT-POK composition further comprises 0-1.5 parts by weight of an auxiliary agent, wherein the auxiliary agent is an antioxidant and / or a lubricant.

[0012] The antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, di[3-(1,1-dimethylethyl)-4-hydroxy-5-methylphenylpropionate]triethylene glycol, pentaerythritol tetrakis(3-laurylthiopropionate) and tris[2,4-di-tert-butylphenyl]phosphite.

[0013] The lubricant is one or more of stearic acid lubricants, montanol wax lubricants, alcohol lubricants, amide lubricants, silicone lubricants and hydrocarbon lubricants. The lubricant is preferably an amide lubricant. The lubricant is more preferably one or more of ethylenebisoctadecanoic acid amide, N,N-ethylenebisstearic acid amide, behenic acid amide, erucic acid amide, oleic acid amide and ethylenebisstearic acid amide.

[0014] Furthermore, the diameter of the glass fiber is 5-20 μm. Further preferably, the glass fiber is a modified glass fiber. Further preferably, the glass fiber is a modified long glass fiber and / or a chopped glass fiber. Further preferably, the glass fiber is a glass fiber modified by a coupling agent; the coupling agent is selected from one or two of a silane coupling agent and a titanate coupling agent. Further preferably, the glass fiber is a chopped glass fiber modified by a silane coupling agent. The glass fiber modified by the coupling agent has better interface properties with the PBT-POK component. The present invention also provides a method for preparing the above-mentioned glass fiber reinforced PBT-POK composition, comprising the following steps:

[0015] S1: weigh and pre-mix the components according to the ratio to obtain a premix;

[0016] S2: putting the premix of step S1 into an extruder, performing melt blending and extrusion granulation to obtain the glass fiber reinforced PBT-POK composition.

[0017] Further, the extruder is a twin-screw extruder, the screw speed of the twin-screw extruder is 250-350 rpm, the barrel temperatures of the twin-screw extruder from the feeding port to the die are 160°C-180°C, 180°C-220°C, 200°C-240°C, 220°C-240°C, 220°C-250°C, 220°C-250°C, 220°C-240°C, 220°C-240°C, 200°C-240°C, 200°C-240°C, the feeding rate is 50kg / h-200kg / h, and the vacuum degree is (-0.1)-0MPa.

[0018] The present invention also provides the use of the glass fiber reinforced PBT-POK composition in the preparation of electronic appliances, household appliances and automobiles, such as the preparation of gears, bearings, electrical appliance / automobile housings and the like.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention improves the thermal stability and wear resistance of the composite material by compounding PBT resin with a specific content of POK resin, and at the same time, calcium sulfate whiskers are added to further enhance the wear resistance of the material, and finally the material has good thermal stability and wear resistance. Under the joint action of the above-mentioned calcium sulfate whiskers, glass fibers and other components of the system, the glass fiber reinforced PBT-POK composition prepared by the present invention has excellent wear resistance and improved warpage. A large amount of experimental data shows that only adding one or two additives or the addition amount is not within the range specified by the present invention is not enough to achieve the performance effect described in the present invention. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] <Preparation of Examples and Comparative Examples>

[0023] The raw materials used in the examples and comparative examples of the present invention are all commercially available, but are not limited to these materials:

[0024] PBT resin A: intrinsic viscosity 0.72, brand GX 111, purchased from Sinopec Yizheng Chemical Fiber;

[0025] PBT resin B: intrinsic viscosity 1.2, brand GL 234, purchased from Sinopec Yizheng Chemical Fiber;

[0026] POK resin A: melt index is 6g / 10min, brand name M630A, purchased from Hyosung, South Korea;

[0027] POK resin B: melt index is 60g / 10min, brand M330A, purchased from Hyosung, South Korea;

[0028] POK resin C: melt index is 200g / 10min, brand M930A, purchased from Hyosung, Korea;

[0029] Calcium sulfate whiskers 1: width 5-15 μm, length 50-200 μm, thickness 0.2-0.8 μm, purchased from Shenzhen Chaobang;

[0030] Calcium sulfate whiskers 2: width 1-4 μm, length 10-40 μm, thickness 0.1±0.05 μm, purchased from Sichuan Wanrun Non-metallic Mineral Materials Co., Ltd.

[0031] Compatibilizer: ethylene-acrylic acid-methacrylate glycidyl ester, brand PTW, purchased from DuPont, USA;

[0032] Glass fiber: brand E7CS10-03-568H, purchased from Changzhou Liantuo Composite Materials Co., Ltd.;

[0033] Antioxidant: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, commercially available, the same commercial product was used in parallel experiments;

[0034] Lubricant: Amide lubricant, commercially available, the same commercial product was used in parallel experiments.

[0035] The preparation methods of the embodiments of the present invention and the comparative examples are as follows:

[0036] S1: According to the ratios in Table 1 and Table 3, weigh and pre-mix the components to obtain a premix;

[0037] S2: The premix of step S1 is put into a twin-screw extruder for melt blending and extrusion granulation to obtain a glass fiber reinforced PBT-POK composition.

[0038] The screw speed of the twin-screw extruder is 300 rpm, and the barrel temperatures from the feeding port to the die are 170°C, 220°C, 240°C, 250°C, 240°C, 220°C, 200°C, 200°C, 220°C, and 240°C, respectively. The feeding rate is 100kg / h and the vacuum degree is -0.1MPa.

[0039] <Test Standard>

[0040] The performance test standards of the embodiments and comparative examples of the present invention are as follows:

[0041] Tensile strength: refer to ISO527 / 2-93 standard;

[0042] Notched impact strength: The test method refers to ISO180-2000 standard;

[0043] Warping performance: After the extruded granulated glass fiber reinforced PET / PBT composite material is dried, it is injection molded into a 60*60*0.8mm square plate (drying conditions are 120℃, 4 hours). The square plate is placed on a flat table and the highest distance between the four corners of the square plate and the table is measured, which is the warping of the square plate. The smaller the distance, the lower the warping, the better the material's anti-warping property, and the lower the degree of deformation of the material after it is made into a product.

[0044] Evaluation of friction coefficient and wear resistance: Friction between plastics, plastic multifunctional friction tester, load 3.88N, rotation speed 200rpm, test time 120min, the equipment records the friction coefficient and tests the wear of the material; between plastic and metal (45# steel), plastic multifunctional friction tester, load 10N, rotation speed 500rpm, test time 120min, the equipment records the friction coefficient and tests the wear of the material;

[0045] Thermal stability: According to GB / T 7141-2008, 150mm*10mm*10mm mechanical specimens were aged in a hot air oven at 150°C. After 500 hours, the specimens were taken out and placed in a constant temperature and humidity environment for 24 hours to test the tensile strength and notched impact strength.

[0046] Table 1. Formula of Examples 1-8 (parts by weight)

[0047]

[0048] Table 2. Performance test results of Examples 1-8

[0049]

[0050]

[0051] Table 3. Comparative Examples 1-6 Formula (parts by weight)

[0052] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 PBT Resin A 100 0 100 100 100 100 100 POK Resin A 0 60 60 60 50 130 60 Compatibilizer 3 3 0 3 3 3 3 Fiberglass 40 40 40 40 40 40 40 Calcium sulfate whiskers 1 10 10 10 25 10 10 Calcium sulfate whiskers 2 10 Antioxidants 1.5 1.5 1.5 1.5 1.5 1.5 1.5

[0053] Table 4. Performance test results of comparative examples 1-6

[0054]

[0055] Compared with Example 1, Comparative Example 1 does not add POK resin, which leads to an increase in the friction coefficient of Comparative Example 1, and an increase in the wear between plastics and between plastics and metals. However, since PBT resin has good thermal stability, the addition of POK resin will reduce the thermal stability of the composition to a certain extent, so the tensile strength and notched impact strength of Comparative Example 1 after aging are less reduced than those of Example 1.

[0056] Compared with Example 1, Comparative Example 2 does not add PBT resin, which leads to a greater decrease in the tensile strength and notched impact strength of Comparative Example 2 after aging, that is, the thermal stability of Comparative Example 2 decreases.

[0057] Compared with Example 1, Comparative Example 3 does not add a compatibilizer, and the thermal stability of Comparative Example 3 is reduced, the friction coefficient and abrasion are increased, and the wear resistance is deteriorated.

[0058] Compared with Example 1, Comparative Example 4 adds excessive calcium sulfate whiskers, and the tensile strength and notched impact strength are significantly inferior to those of Example 1. In addition, the wear between plastics and the wear between plastics and metals in Comparative Example 4 are increased, the friction coefficient between plastics and metals is increased, and the wear resistance is reduced.

[0059] Compared with Example 1, in Comparative Examples 5 and 6, the amount of POK resin added in Comparative Examples 5 and 6 is excessive or too little, and the decrease in the tensile strength and notched impact strength of Comparative Examples 5 and 6 after aging is increased.

[0060] Compared with Example 1, Comparative Example 7 adds calcium sulfate whiskers 2, and the wear resistance effect is far inferior to Example 1, and the warpage is also much higher than Example 1.

[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A glass fiber reinforced PBT-POK composition, It is characterized in that By weight, it includes the following components: PBT resin 100 parts; 60-120 parts of POK resin; 3-8 parts of compatibilizer; Glass fiber 40-80 parts; Calcium sulfate whiskers 10-20 parts; The compatibilizer is ethylene-acrylic acid-glycidyl methacrylate; The width of the calcium sulfate whisker is 5-15 μm, and the thickness of the calcium sulfate whisker is 0.2-0.8 μm; The diameter of the glass fiber is 5-20 μm.

2. The glass fiber reinforced PBT-POK composition according to claim 1, It is characterized in that The melt index of the POK resin is 6-200 g / 10 min.

3. The glass fiber reinforced PBT-POK composition according to claim 2, It is characterized in that The melt index of the POK resin is 10-150 g / 10 min.

4. The glass fiber reinforced PBT-POK composition according to claim 3, It is characterized in that The melt index of the POK resin is 20-120 g / 10 min.

5. The glass fiber reinforced PBT-POK composition according to claim 4, It is characterized in that The melt index of the POK resin is 30-100 g / 10 min.

6. The glass fiber reinforced PBT-POK composition according to claim 1, It is characterized in that The intrinsic viscosity of the PBT resin is 0.72-1.2 dL / g.

7. The glass fiber reinforced PBT-POK composition according to claim 1, It is characterized in that The glass fiber reinforced PBT-POK composition further comprises 0-1.5 parts by weight of an auxiliary agent, wherein the auxiliary agent is an antioxidant and / or a lubricant.

8. A method for preparing the glass fiber reinforced PBT-POK composition according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1: According to the ratio, weigh and pre-mix the components to obtain a premix; S2: putting the premix of step S1 into an extruder, performing melt blending and extrusion granulation to obtain the glass fiber reinforced PBT-POK composition.

9. The method for preparing the glass fiber reinforced PBT-POK composition according to claim 8, It is characterized in that The extruder is a twin-screw extruder, and the screw speed of the twin-screw extruder is 250-350 rpm.

10. Use of the glass fiber reinforced PBT-POK composition according to any one of claims 1 to 7 in the preparation of electronic appliances, household appliances and automobiles.