A kind of light real stone paint and preparation method thereof

By using a formula of sepiolite and chitosan film combined with nanoscale organic montmorillonite and carboxymethyl cellulose in water-based real stone paint, the problem that the water-based real stone paint is easy to crack and fall off under low temperature conditions has been solved, and the problem has been achieved. Better temperature regulation and adhesion significantly improve the stability and construction performance of the coating.

CN116376381BActive Publication Date: 2024-10-15TIANJIN DEPUWEI COATINGS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310371753.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

The coating of existing water-based real stone paint is easy to crack and fall off under low temperature conditions, which affects the construction process and the beauty of the building.

Method used

Using a lightweight real stone paint formula, including base paint, granulation liquid, continuous phase solution and white sand, the sepiolite is filled with paraffin and chitosan membranes through ultrasonic oscillation to form a phase change material capsule, combined with nanoscale organic montmorillonite and carboxyl Methylcellulose improves the temperature regulation and adhesion of the coating and reduces the impact of low temperature.

Benefits of technology

Significantly reduces the cracking and peeling of the coating under low temperature conditions, shortens the film formation time, improves the adhesion and firmness of the coating, and maintains the integrity of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004168826660000051
    Figure BDA0004168826660000051
  • Figure BDA0004168826660000061
    Figure BDA0004168826660000061
  • Figure BDA0004168826660000062
    Figure BDA0004168826660000062
Patent Text Reader

Abstract

The present application relates to the field of lightweight real stone paint, and specifically discloses a lightweight real stone paint and a preparation method thereof. The lightweight real stone paint includes the following raw materials in parts by weight: 250-270 parts of base paint, 120-130 parts of granulation liquid, 130-150 parts of continuous phase solution and 450-500 parts of white sand; the continuous phase solution includes the following raw materials in parts by weight: 200-220 parts of water, 200-300 parts of epoxy resin emulsion, 350-450 parts of acrylic resin emulsion, 100-150 parts of pure acrylic resin emulsion, 1-2 parts of preservative, 1-2 parts of thickener, 30-40 parts of film-forming aid, 1-2 parts of cellulose ether and 150-200 parts of phase change material capsules; in addition, the lightweight real stone paint prepared by the present application has the advantages of good low-temperature adhesion, good low-temperature film-forming property and the coating is not easy to crack and fall off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coatings, and more specifically, to a lightweight true stone paint and a preparation method thereof. Background Art

[0002] Water-based paint is a paint that uses water as a dispersion medium and diluent. Compared with organic solvent-based paint, water-based paint saves a lot of organic material resources, greatly reduces the pollution of the atmosphere caused by the volatilization of organic solvents in the paint and the fire hazard during the construction process. Water is an extremely abundant resource on the earth. It is easy to use and low in cost. When used as a solvent in paint, it will not damage or cause less damage to water resources. Therefore, water-based paint not only reduces the emission of volatile organic solvents, but also saves resources and energy, and is convenient for transportation and storage. With the enhancement of people's environmental awareness, the use of water-based paint has increased year by year, and has gradually become the mainstream direction of the development of the modern paint industry.

[0003] Water-based real stone paint is a building paint with a stone decorative effect on the surface of a building, which is made of acrylic resin emulsion as the main film-forming material, stone crushed stones of various colors and particle sizes as aggregates, and various additives. It is used more and more widely in buildings because of its low resource consumption, easy construction, no safety hazards, rich colors and varieties. However, most of the water-based real stone paints currently used in the market have poor antifreeze effects. In low-temperature areas in winter, especially in the northeast, the water-based real stone paint is affected by the low temperature and takes a long time to dry when forming a film. The paint layer is prone to cracking and falling off, affecting the construction process and the beauty of the building. Summary of the invention

[0004] In order to reduce the cracking and shedding of the coating of water-based real stone paint under low temperature conditions, the present application provides a lightweight real stone paint and a preparation method thereof.

[0005] In the first aspect, the present application provides a lightweight real stone paint, which adopts the following technical solution:

[0006] A light real stone paint comprises the following raw materials in parts by weight: 250-270 parts of base paint, 120-130 parts of granulation liquid, 130-150 parts of continuous phase solution and 450-500 parts of white sand;

[0007] The continuous phase solution comprises the following raw materials in parts by weight: 200-220 parts of water, 200-300 parts of epoxy resin emulsion, 350-450 parts of acrylic resin emulsion, 100-150 parts of pure acrylic resin emulsion, 1-2 parts of preservative, 1-2 parts of thickener, 30-40 parts of film-forming aid, 1-2 parts of cellulose ether and 150-200 parts of phase change material capsules;

[0008] The phase change material capsule comprises the following preparation steps:

[0009] S1: Immerse the sepiolite in paraffin and oscillate ultrasonically for 30-50 minutes;

[0010] S2: Take out the meerschaum and place it at low temperature until the paraffin solidifies;

[0011] S3: immersing the sepiolite in a chitosan solution with a mass fraction of 3-5%, and forming a chitosan film on the surface of the sepiolite after drying to obtain a phase change material capsule.

[0012] By adopting the above technical solution, the present application uses super base paint, granulation liquid, continuous phase solution and white sand to prepare lightweight real stone paint. The present application uses a small amount of white sand, which can significantly reduce the coating load, thereby reducing the cracking and shedding of the coating under low temperature conditions;

[0013] The internal pores of sepiolite are large, and the thermal conductivity is high. When sepiolite is combined with the coating, the coating seals the pores on the surface of the sepiolite, which can lock the air inside the sepiolite, play a role in heat preservation, and reduce the impact of low temperature on the coating. In addition, sepiolite is light in weight and can also replace sand and gravel. When used together with white sand, it can reduce the coating load.

[0014] Fill paraffin wax into the pores of sepiolite. Paraffin wax can make reversible changes between solid-solid and solid-liquid according to the changes in the external temperature of the environment, absorb or release heat, and form a "constant climate microenvironment" in the coating, thereby realizing the temperature regulation function and reducing the impact of low temperature on the coating. The outer layer of sepiolite is also wrapped with chitosan film. On the one hand, the chitosan film can cooperate with the coating to form a "double-layer blockade" for paraffin to prevent paraffin leakage. On the other hand, chitosan molecules contain a large number of hydroxyl and carboxyl groups, which can cross-link with the functional groups of epoxy resin, acrylic resin and pure acrylic resin, thereby improving the firmness of sepiolite in the coating and reducing the possibility of sepiolite falling off the coating due to low temperature, thereby maintaining the integrity of the coating.

[0015] Preferably, the cellulose ether is carboxymethyl cellulose, and the raw materials of the continuous phase solution further include 5-8 parts by weight of organic montmorillonite.

[0016] By adopting the above technical scheme, the nano-scale organic montmorillonite lamellar structure is introduced into the resin emulsion in the present application. On the one hand, the "maze effect" of the lamellar structure of the montmorillonite itself can accommodate more gas and play a role in thermal insulation of the coating. The organic montmorillonite can also improve the anti-settling performance, anti-syneresis performance and anti-splashing properties of the coating. Carboxymethyl cellulose can quickly associate with the pure acrylic emulsion to further enhance the internal adhesion and strength of the paint film. The combination of organic montmorillonite and carboxymethyl cellulose can increase the volatilization rate of water and shorten the film-forming time, thereby reducing the possibility of cracking of the coating during construction at low temperatures.

[0017] Preferably, the mass ratio between the carboxymethyl cellulose and the organic montmorillonite is 1:(4-5).

[0018] By adopting the above technical solution, the application further optimizes the mass ratio of carboxymethyl cellulose and organic montmorillonite, which can further exert the synergistic effect between each other, significantly shorten the film formation time, and reduce low-temperature cracking of the coating.

[0019] Preferably, the raw materials of the continuous phase solution further include 4-6 parts by weight of monoalkoxy pyrophosphate.

[0020] By adopting the above technical scheme, the monoalkoxy group reacts with the hydroxyl group on the chitosan to form a chemical bond, and can also produce chemical bonding at the interface of white sand, organic montmorillonite and matrix resin to reduce particle shedding. The pyrophosphate group can decompose to form a phosphate group, which combines with the latex particles to strengthen the interlayer cohesion and reduce the shedding of the low-temperature coating.

[0021] Preferably, the particle size of the sepiolite is 0.5-5 mm.

[0022] By adopting the above technical solution, if the particle size of the sepiolite is too small, the loaded paraffin is small, and it is difficult to regulate the coating temperature; if the particle size of the sepiolite is too large, it is easy to fall off from the coating.

[0023] Preferably, the raw materials of the continuous phase solution further include 1-2 parts by weight of ethyl silicate.

[0024] By adopting the above technical solution, ethyl silicate can form a mesh structure after drying, connecting the coating and the building exterior wall, which can improve the adhesion of the coating. The synergistic effect of ethyl silicate and carboxymethyl cellulose can reduce the surface tension of the coating, making the coating easier to adhere to the wall surface, while further exerting the performance of silica sol to improve the adhesion between the coating and the building exterior wall.

[0025] Preferably, the film-forming aid comprises alcohol ester and ethylene glycol.

[0026] By adopting the above technical solution, the combination of alcohol ester dodecaned and ethylene glycol can quickly increase the speed of coating film formation at low temperatures and reduce the possibility of cracks in the coating due to the difficulty of volatilization of water in the low-temperature system and freezing.

[0027] In a second aspect, the present application provides a method for preparing a lightweight real stone paint, using the following technical solution:

[0028] A method for preparing a lightweight real stone paint comprises the following steps:

[0029] S1: mixing the base paint and the granulation liquid, and granulating to obtain a mixed solution A;

[0030] S2: adding the continuous phase solution to the above mixed solution and stirring evenly to obtain a mixed solution B;

[0031] S3: Add white sand into the mixed solution B and mix evenly to obtain a light-weight real stone paint.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. The present application adopts super base paint, granulation liquid, continuous phase solution and white sand to prepare lightweight real stone paint. The present application uses a small amount of white sand, which can significantly reduce the coating load, thereby reducing the cracking and shedding of the coating under low temperature conditions; the present application fills paraffin wax inside the pores of sepiolite to form a "constant climate microenvironment" in the coating, thereby realizing the temperature regulation function and reducing the impact of low temperature on the coating. The outer layer of sepiolite is also wrapped with a chitosan film. On the one hand, the chitosan film can cooperate with the coating to form a "double-layer blockade" for paraffin wax to prevent paraffin leakage. On the other hand, the chitosan molecule contains a large number of hydroxyl and carboxyl groups, which can be cross-linked with the functional groups of epoxy resin, acrylic resin and pure acrylic resin, thereby improving the firmness of sepiolite in the coating and reducing the possibility of sepiolite falling off the coating due to low temperature, thereby maintaining the integrity of the coating;

[0034] 2. The present application introduces nano-scale organic montmorillonite sheet structure into the resin emulsion in the present application, which can play a role in thermal insulation of the coating. Carboxymethyl cellulose can quickly associate with the pure acrylic emulsion to further enhance the internal adhesion and strength of the paint film. The combination of organic montmorillonite and carboxymethyl cellulose can increase the volatilization rate of water and shorten the film-forming time, thereby reducing the possibility of cracking of the coating during construction at low temperatures.

[0035] 3. Ethyl silicate is also added in this application. After drying, ethyl silicate can form a mesh structure, which connects the coating and the building exterior wall and improves the adhesion of the coating. The synergistic effect of ethyl silicate and carboxymethyl cellulose can reduce the surface tension of the coating, making the coating easier to fit the wall surface, while further exerting the performance of silica sol to improve the adhesion between the coating and the building exterior wall. DETAILED DESCRIPTION

[0036] Source of raw materials:

[0037] The sepiolite comes from Hunan Lihengtong New Materials Co., Ltd.;

[0038] Chitosan was from Weifang Kehai Chitosan Co., Ltd.;

[0039] Epoxy resin emulsion was from Shanghai Yueyi Chemical Co., Ltd., model CYDW-112W50;

[0040] Acrylic resin emulsion was from Jining Huakai Resin Co., Ltd., model 8019;

[0041] Pure acrylic resin emulsion was from Zhengzhou Yiteng Chemical Products Co., Ltd., model 707;

[0042] The preservative was from Thor, UK, model MBS5050;

[0043] The thickener is from Dow Chemical, model TT935;

[0044] Organic montmorillonite was from Guangying New Materials (Guangzhou) Co., Ltd., model TY-788C;

[0045] Monoalkoxy pyrophosphate was from Kenrich Petrochemical Company, USA, model KR-12;

[0046] Ethyl silicate was from Shanghai Gaoming Chemical Co., Ltd., model 963258;

[0047] Hydroxyethyl cellulose and carboxymethyl cellulose were from Shanghai Yuanye Biotechnology Co., Ltd.

[0048] The present application is further described in detail below in conjunction with preparation examples and embodiments.

[0049] Preparation Example

[0050] Preparation Example 1

[0051] The phase change material capsule comprises the following preparation steps:

[0052] S1: immerse sepiolite with a particle size of 0.5-5 mm in paraffin and ultrasonically vibrate for 30 min;

[0053] S2: Take out the meerschaum and place it at low temperature until the paraffin solidifies;

[0054] S3: immersing the sepiolite in a chitosan solution with a mass fraction of 3%, and forming a chitosan film on the surface of the sepiolite after drying to obtain a phase change material capsule.

[0055] Preparation Example 2

[0056] The phase change material capsule comprises the following preparation steps:

[0057] S1: immerse sepiolite with a particle size of 0.5-5 mm in paraffin and ultrasonically vibrate for 40 min;

[0058] S2: Take out the meerschaum and place it at low temperature until the paraffin solidifies;

[0059] S3: immersing the sepiolite in a chitosan solution with a mass fraction of 4%, and forming a chitosan film on the surface of the sepiolite after drying to obtain a phase change material capsule.

[0060] Preparation Example 3

[0061] The phase change material capsule comprises the following preparation steps:

[0062] S1: immerse sepiolite with a particle size of 0.5-5 mm in paraffin and ultrasonically vibrate for 50 min;

[0063] S2: Take out the meerschaum and place it at low temperature until the paraffin solidifies;

[0064] S3: immersing the sepiolite in a chitosan solution with a mass fraction of 5%, and forming a chitosan film on the surface of the sepiolite after drying to obtain a phase change material capsule.

[0065] Preparation Example 4

[0066] The difference between Preparation Example 4 and Preparation Example 1 is that the particle size of the sepiolite is 0.1-0.5 mm, and the remaining steps are the same as Preparation Example 1.

[0067] Preparation Example 5

[0068] The difference between Preparation Example 5 and Preparation Example 1 is that the particle size of the sepiolite is 5-10 mm, and the remaining steps are the same as Preparation Example 1.

[0069] Preparation Example 6

[0070] The difference between Preparation Example 6 and Preparation Example 1 is that the surface of the sepiolite does not undergo the S3 step, and the remaining steps are the same as those in Preparation Example 1.

[0071] Preparation Example 7

[0072] The difference between Preparation Example 7 and Preparation Example 1 is that the chitosan solution with a mass fraction of 4% is replaced by a starch solution with a mass fraction of 50%, and the remaining steps are the same as those of Preparation Example 1.

[0073] Preparation Example 8

[0074] The raw materials and dosage of the base paint are shown in Table 1, and the preparation method is as follows:

[0075] S1: Mix the lithium magnesium silicate protective colloid and water according to the amount and disperse them at a high speed (1000r / min) for 40 minutes to prepare a 10% lithium magnesium silicate protective colloid aqueous solution for use;

[0076] S2: Add water, long-term preservative, dispersant and defoamer into a mixing tank in order, at a speed of 300 r / min, and mix well;

[0077] S3: Add titanium dioxide and kaolin in order and disperse for 5 minutes at a speed of 800 r / min;

[0078] S4: Add hydroxyethyl cellulose according to the amount and continue dispersing for 5 minutes at a speed of 1000 r / min;

[0079] S5: Ethylene glycol, film-forming agent and multifunctional additive are added in order and dispersed for 10 minutes at a speed of 1200 r / min;

[0080] S6: Reduce the speed to 800r / min, and then add pure acrylic emulsion according to the amount;

[0081] S7: Add defoamer and bactericide in order, with a rotation speed of 1300r / min;

[0082] S8: slowly add the 10% lithium magnesium silicate protective glue solution prepared in advance in step 1 at a rotation speed of 1300 r / min;

[0083] S9: Add thickeners in order according to the amount, with the rotation speed being 1100r / min, to obtain the base paint.

[0084] Table 1 Raw materials and dosage of real stone paint base paint

[0085]

[0086]

[0087] Preparation Example 9

[0088] The raw materials and dosage of the granulation liquid are shown in Table 2, and the preparation method is as follows:

[0089] S1: Add water into the mixing tank according to the amount and disperse at low speed, with a speed of 400r / min.

[0090] S2: Slowly add the long-acting preservative, lithium magnesium silicate protective gel, xanthan gum and carboxymethyl cellulose in order, adjust the speed to 500r / min, disperse for 3 minutes, increase the dispersion speed to 1000r / min, and disperse for 10 minutes.

[0091] S3: Add the multifunctional additive according to the amount and continue to disperse at high speed for 20 minutes at a speed of 1300r / min.

[0092] S4: Add the fungicide and water slowly in order according to the amount. During the addition, the rotation speed is slowly reduced to 300r / min. Disperse at low speed for 5 minutes to obtain granulation liquid.

[0093] Table 2 Granulation liquid raw materials and their dosage

[0094]

[0095]

[0096] Example

[0097] Example 1

[0098] A method for preparing a lightweight real stone paint comprises the following steps:

[0099] S1: 250 kg of base paint was mixed with 120 kg of granulation liquid, and granulated to obtain a mixed solution A;

[0100] S2: Add 130 kg of the continuous phase solution into the mixed solution A and stir evenly to obtain a mixed solution B;

[0101] S3: Add 450 kg of white sand (250 kg of 80-120 mesh white sand, 200 kg of 40-80 mesh white sand) into the mixed solution B and mix evenly to obtain a light-weight real stone paint.

[0102] The base paint is from Preparation Example 8, and the granulation liquid is from Preparation Example 9;

[0103] The continuous phase solution is prepared by mixing the following raw materials: 200 kg of water, 200 kg of epoxy resin emulsion, 350 kg of acrylic resin emulsion, 100 kg of pure acrylic resin emulsion, 1 kg of preservative, 1 kg of thickener, 30 kg of film-forming aid (15 kg of alcohol ester and 15 kg of ethylene glycol), 1 kg of carboxymethyl cellulose, 5 kg of organic montmorillonite, 4 kg of monoalkoxy pyrophosphate, 1 kg of ethyl silicate and 150 kg of phase change material capsules; wherein the phase change material capsules come from Preparation Example 1.

[0104] Example 2

[0105] A method for preparing a lightweight real stone paint comprises the following steps:

[0106] S1: 260 kg of base paint was mixed with 125 kg of granulation liquid, and granulated to obtain a mixed solution A;

[0107] S2: Add 140 kg of the continuous phase solution into the mixed solution A and stir evenly to obtain a mixed solution B;

[0108] S3: Add 470 kg of white sand (260 kg of 80-120 mesh white sand, 210 kg of 40-80 mesh white sand) into the mixed solution B and mix evenly to obtain a light-weight real stone paint.

[0109] The base paint comes from 8, and the granulation liquid comes from Preparation Example 9;

[0110] The continuous phase solution is prepared by mixing the following raw materials: 210 kg of water, 250 kg of epoxy resin emulsion, 400 kg of acrylic resin emulsion, 120 kg of pure acrylic resin emulsion, 1.5 kg of preservative, 1.5 kg of thickener, 35 kg of film-forming aid (20 kg of alcohol ester and 15 kg of ethylene glycol), 1.5 kg of carboxymethyl cellulose, 6.5 kg of organic montmorillonite, 5 kg of monoalkoxy pyrophosphate, 1.5 kg of ethyl silicate and 170 kg of phase change material capsules; wherein the phase change material capsules are from Preparation Example 1.

[0111] Example 3

[0112] A method for preparing a lightweight real stone paint comprises the following steps:

[0113] S1: 270 kg of base paint was mixed with 130 kg of granulation liquid, and granulated to obtain a mixed solution A;

[0114] S2: Add 150 kg of the continuous phase solution into the mixed solution A and stir evenly to obtain a mixed solution B;

[0115] S3: Add 500 kg of white sand (270 kg of 80-120 mesh white sand, 230 kg of 40-80 mesh white sand) into the mixed solution B and mix evenly to obtain a light-weight real stone paint.

[0116] The base paint is from Preparation Example 8, and the granulation liquid is from Preparation Example 9;

[0117] The continuous phase solution is prepared by mixing the following raw materials: 220 kg of water, 300 kg of epoxy resin emulsion, 450 kg of acrylic resin emulsion, 150 kg of pure acrylic resin emulsion, 2 kg of preservative, 2 kg of thickener, 40 kg of film-forming aid (20 kg of alcohol ester and 15 kg of ethylene glycol), 2 kg of carboxymethyl cellulose, 8 kg of organic montmorillonite, 6 kg of monoalkoxy pyrophosphate, 2 kg of ethyl silicate and 200 kg of phase change material capsules; wherein the phase change material capsules are from Preparation Example 1.

[0118] Example 4

[0119] The difference between Example 4 and Example 2 is that the amount of organic montmorillonite added is 6 kg, and the remaining steps are the same as Example 2.

[0120] Example 5

[0121] The difference between Example 5 and Example 2 is that the amount of organic montmorillonite added is 7.5 kg, and the remaining steps are the same as Example 2.

[0122] Example 6

[0123] The difference between Example 6 and Example 2 is that the amount of organic montmorillonite added is 5.8 kg, and the remaining steps are the same as Example 2.

[0124] Example 7

[0125] The difference between Example 7 and Example 2 is that the amount of organic montmorillonite added is 7.7 kg, and the remaining steps are the same as Example 2.

[0126] Example 8

[0127] The difference between Example 8 and Example 2 is that carboxymethyl cellulose is replaced by an equal amount of hydroxyethyl cellulose, and the remaining steps are the same as Example 2.

[0128] Example 9

[0129] The difference between Example 9 and Example 2 is that the organic montmorillonite is replaced by an equal amount of diatomaceous earth, and the remaining steps are the same as those of Example 2.

[0130] Example 10

[0131] The difference between Example 10 and Example 2 is that monoalkoxy pyrophosphate is not added to the continuous phase solution, and the remaining steps are the same as those in Example 2.

[0132] Embodiment 11

[0133] The difference between Example 11 and Example 2 is that the monoalkoxy pyrophosphate is replaced by an equal amount of KH550 silane coupling agent, and the remaining steps are the same as Example 2.

[0134] Example 12

[0135] The difference between Example 12 and Example 2 is that ethyl silicate is not added to the continuous phase solution, and the remaining steps are the same as Example 2.

[0136] Example 13

[0137] The difference between Example 13 and Example 2 is that ethylene glycol is replaced by an equal amount of alcohol ester twelve, and the remaining steps are the same as Example 2.

[0138] Embodiment 14

[0139] The difference between Example 14 and Example 2 is that the alcohol ester is replaced by an equal amount of ethylene glycol, and the remaining steps are the same as Example 2.

[0140] Examples 15-20

[0141] The difference between Examples 15-20 and Example 2 is that the phase change material capsules are respectively from Preparation Examples 2-7, and the remaining steps are the same as Example 2.

[0142] Comparative Example

[0143] Comparative Example 1

[0144] The difference between Comparative Example 1 and Example 2 is that no phase change material capsules are added, and the remaining steps are the same as those of Example 2.

[0145] Performance testing

[0146] Detection Methods

[0147] Low-temperature film-forming performance test: According to the "Synthetic Quality Emulsion Sand-walled Architectural Coatings" JG / T24-2018, mortar test blocks were prepared. The low-temperature film-forming test was carried out in an environment of -25°C. The real stone paints in Examples 1-20 and Comparative Example 1 were applied to the mortar test blocks. After 5 hours, the film formation was observed by professionals. If the film is formed normally, the surface will be slightly sticky when touched by a finger, but there will be no paint sticking to the finger, and there will be basically no traces of the base material on the surface; otherwise, there will be obvious traces of the base material on the surface, and it will be white.

[0148] Real stone paint bonding strength test and coating state test experiment: The real stone paint in Examples 1-20 and Comparative Example 1 was applied to the mortar test block, and the bonding strength was tested according to the bonding strength method under standard conditions in "Synthetic Quality Emulsion Sand Wall Architectural Coating" JG / T24-2018. The test blocks coated with the real stone paint in Examples 1-20 and Comparative Example 1 and after curing were subjected to freeze-thaw cycles in a freeze-thaw cycle tester, and each cycle included freezing at -35°C for 2h, then warming to 5°C and soaking in water for 2h. For the test blocks subjected to 20, 60, and 100 freeze-thaw cycles, the test blocks were tested according to the bonding strength test method in "Synthetic Resin Emulsion Sand Wall Architectural Coating" JG / T24-2018, and the coatings that had undergone 100 freeze-thaw cycle experiments were observed to see if there was peeling or cracking; for the test blocks that had undergone 100 freeze-thaw cycles, a plastic scraper was used to scrape the coating surface to see if the sepiolite particles in the coating had fallen off. The specific experimental results are shown in Table 3:

[0149] Table 3 Real stone paint coating state, film forming state and bonding strength data prepared in Examples 1-20 and Comparative Example 1

[0150]

[0151]

[0152]

[0153] Combining the data of Examples 1-3 and Table 1, it can be seen that the low-temperature film-forming performance of the lightweight real stone paint prepared in Examples 1-3 is good, and no obvious traces of the base material are observed on the surface. After 100 freeze-thaw cycles, the test block has a bonding strength greater than 1.04MPa, and the coating subjected to 100 freeze-thaw cycles has no cracks or peeling, and the sepiolite in the coating is still firm in the coating without sand falling;

[0154] Combining the data of Example 2, Examples 4-9 and Table 1, it can be seen that the combination of organic montmorillonite and carboxymethyl cellulose can increase the volatilization rate of water, shorten the film-forming time, enhance the low-temperature adhesion of the coating, and reduce the possibility of cracking and falling off of the coating during construction at low temperatures. In addition, when the mass ratio between carboxymethyl cellulose and organic montmorillonite is 1:(4-5), the synergistic effect between them can be further exerted to jointly improve the low-temperature bonding effect of the coating;

[0155] Combining the data of Example 2, Examples 10-11 and Table 1, it can be seen that, compared with common coupling agents, such as silane coupling agents, monoalkoxy pyrophosphate can effectively improve the low-temperature adhesion of the coating and reduce delamination cracking and particle shedding. This is mainly because the monoalkoxy reacts with the hydroxyl group on the chitosan to form a chemical bond, thereby enhancing the bonding force between the coating and the sepiolite and reducing particle shedding. The pyrophosphate group can decompose to form a phosphate group, which combines with the latex particles to strengthen the interlayer cohesion, enhance the low-temperature bonding force between the coating and the substrate, and reduce the shedding of the low-temperature coating.

[0156] Combining the data of Example 2, Examples 12-14 and Table 1, it can be seen that ethyl silicate and carboxymethyl cellulose can synergistically reduce the surface tension of the coating, making the coating easier to adhere to the wall surface, while further exerting the performance of silica sol to improve the low-temperature adhesion between the coating and the substrate;

[0157] Combining the data of Example 2, Examples 17-18 and Table 1, it can be seen that when the particle size of sepiolite is too small, the load of paraffin is small, and it is difficult to control the coating temperature. When the particle size of sepiolite is too large, it is easy to fall off from the coating. Therefore, when the particle size of sepiolite is 0.5-5 mm, the low-temperature adhesion of the coating can be effectively improved.

[0158] Combined with the data in Example 2, Examples 19-20 and Table 1, it can be seen that the chitosan film on the surface of sepiolite can improve the firmness of sepiolite in the coating and reduce the possibility of sepiolite falling off the coating due to low temperature, thereby maintaining the integrity of the coating; Combined with the data in Example 2, Comparative Example 1 and Table 1, it can be seen that the phase change material capsules prepared in the present application are added to the real stone paint, which is beneficial to the film forming property of the coating, and can effectively reduce the influence of low temperature on the coating, thereby improving the adhesion between the coating and the substrate, thereby reducing the cracking and falling off of the coating.

[0159] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A lightweight real stone paint, Features : comprising the following raw materials in parts by weight: 550-560 parts of base paint, 270-280 parts of granulation liquid, 100-120 parts of continuous phase solution and 100-150 parts of rock flakes; The continuous phase solution comprises the following raw materials in parts by weight: 200-220 parts of water, 200-300 parts of epoxy resin emulsion, 350-450 parts of acrylic resin emulsion, 100-150 parts of pure acrylic resin emulsion, 1-2 parts of preservative, 1-2 parts of thickener, 30-40 parts of film-forming aid, 1-2 parts of cellulose ether and 150-200 parts of phase change material capsules; The phase change material capsule comprises the following preparation steps: S1: Immerse the sepiolite in paraffin and oscillate ultrasonically for 30-50 minutes; S2: Take out the meerschaum and place it at low temperature until the paraffin solidifies; S3: immersing the sepiolite in a chitosan solution having a mass fraction of 3-5%, and forming a chitosan film on the surface of the sepiolite after drying to obtain a phase change material capsule; The cellulose ether is carboxymethyl cellulose, and the raw materials of the continuous phase solution also include 5-8 parts by weight of organic montmorillonite; The raw materials of the continuous phase solution also include 4-6 parts by weight of monoalkoxy pyrophosphate; The particle size of the sepiolite is 0.5-5 mm; The raw materials of the continuous phase solution also include 1-2 parts by weight of ethyl silicate; The acrylic resin emulsion is from Jining Huakai Resin Co., Ltd., brand Archsol8019; The pure acrylic emulsion comes from Zhengzhou Yiteng Chemical Products Co., Ltd., model 707.

2. The lightweight real stone paint according to claim 1, Features: The mass ratio between the carboxymethyl cellulose and the organic montmorillonite is 1:(4-5).

3. The lightweight real stone paint according to claim 1, Features: The film-forming aids include alcohol esters and ethylene glycol.

4. A method for preparing the lightweight true stone paint according to any one of claims 1 to 3, Features: The following steps are involved: S1: mixing the base paint and the granulation liquid, and granulating to obtain a mixed solution A; S2: adding the continuous phase solution to the above mixed solution and stirring evenly to obtain a mixed solution B; S3: Add the rock flakes into the mixed solution B and mix evenly to obtain a light-weight real stone paint.