Lithium aluminum silicate glass and preparation method thereof
By using lithium aluminosilicate glass with a specific component ratio and preparation method in high-end cover glass, the duration of the high point area of Na-CS30 and Na-Dol is extended, and the lithium-sodium ion exchange stress in the existing technology is solved. and depth attenuation problems, improving the sandpaper drop resistance and production stability of the glass.
Patent Information
- Application Number
- CN202310415210.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-18
AI Technical Summary
During the tempering process of existing high-end cover glass, the stress and depth of lithium-sodium ion exchange are prone to attenuation, causing micro-cracks to appear in the glass in a stress-relaxed state, reducing the sandpaper drop resistance, and it is difficult to determine Na-CS30 and Na- The duration of the high point area of Dol affects the stability of glass performance.
Provided is a lithium aluminosilicate glass and a preparation method thereof, by using aluminosilicate glass with a specific component ratio, including SiO2, Al2O3, Li2O, Na2O, K2O, MgO, CaO, B2O3, ZrO 2 and ZnO, using high-temperature melting and tempering processes, controlling the (Li+Na+P+Al)/(Mg+Ca+Zn+B) ratio <4, extending the duration of the high point areas of Na-CS30 and Na-Dol .
It effectively avoids micro-cracks caused by stress relaxation during the tempering process, improves the sandpaper drop resistance of the glass, reduces the time and economic costs of the exploration phase, and makes glass production more stable.
Smart Images

Figure BDA0004184708320000081 
Figure BDA0004184708320000091 
Figure BDA0004184708320000092
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass production and manufacturing, and in particular to lithium aluminum silicate glass and a preparation method thereof. Background Art
[0002] In order to obtain higher sandpaper drop resistance, the ion exchange depth of the high-end cover glass on the market is getting higher and higher during the tempering process. Glass often presents an over-strengthened state, that is, a stress relaxation state, during the ion exchange process. After the ion exchange reaches a certain level, the stress (Na-CS30) and exchange depth (Na-Dol) of lithium-sodium ion exchange will decay as a whole. In the stress relaxation state, a large number of microcracks are prone to appear on the glass, resulting in a decrease in the sandpaper drop resistance of the glass.
[0003] In order to avoid the attenuation of Na-CS30 and Na-Dol, cover panel manufacturers or R&D units often need to conduct a large number of experiments to determine the high points of Na-CS30 and Na-Dol after obtaining a new glass. However, most glasses only last for a short time in the high point area, which makes it difficult to determine the high point. At the same time, it is easy to cause micro cracks in the glass after the attenuation of Na-CS30 and Na-Dol, thereby reducing the glass's anti-sandpaper drop performance.
[0004] Therefore, there is an urgent need for a glass that can last longer in the Na-CS30 and Na-Dol high point areas, which can help technicians find the performance limits of the glass more quickly, reduce the time and economic costs of the exploration phase, make the glass production and performance more stable, and at the same time ensure the glass's resistance to sandpaper drops. Summary of the invention
[0005] Based on this, it is necessary to provide a lithium aluminum silicate glass with a longer duration of Na-CS30 and Na-Dol high point regions and a preparation method thereof.
[0006] In one aspect of the present invention, a lithium aluminosilicate glass is provided. The components of the aluminosilicate glass include, by mass fraction, 48-68% SiO2, 16%≤Al2O3<23%, 2%≤Li2O<4%, 2-9% Na2O, 0.5-4% K2O, 1-6% MgO, 0-4% CaO, 3-8% B2O3, 0-2% P2O5, 0.1-4% ZrO2 and 0-3% ZnO.
[0007] In one embodiment, the components of the lithium aluminosilicate glass include, by mass fraction, 56% to 68% SiO2, 16% to 22% Al2O3, 2% to 3.9% Li2O, 2% to 6% Na2O, 1% to 2.5% K2O, 1% to 4% MgO, 0.1% to 4% CaO, 3% to 5% B2O3, 0.1% to 2% P2O5, 0.1% to 3% ZrO2 and 0.1% to 3% ZnO.
[0008] In one embodiment, the components of the lithium aluminosilicate glass include, by mass fraction, 60% to 65% SiO2, 17% to 21% Al2O3, 3% to 3.9% Li2O, 2% to 4% Na2O, 1% to 2% K2O, 2% to 4% MgO, 0.1% to 3% CaO, 3% to 4.5% B2O3, 0.5% to 2% P2O5, 0.1% to 2% ZrO2 and 0.5% to 3% ZnO.
[0009] In one embodiment, in terms of mass fraction, (Li+Na+P+Al) / (Mg+Ca+Zn+B)<4.
[0010] In another aspect of the present invention, there is provided a method for preparing the lithium aluminosilicate glass, comprising the following steps:
[0011] Weigh the raw materials according to the components, heat to 1600° C. to 1800° C., and keep the temperature for 6 h to 8 h to prepare a molten liquid;
[0012] forming, annealing and cooling the molten liquid to prepare a precursor glass;
[0013] The precursor glass is tempered to prepare the lithium aluminum silicate glass.
[0014] In one embodiment, the annealing conditions include: annealing temperature is T, time is 2h~4h, where T=T g +(30℃~50℃),T g is the glass transition temperature.
[0015] In one embodiment, the cooling step includes: cooling to the glass strain point temperature at a cooling rate of 1°C / min to 2°C / min, and then cooling to room temperature in the furnace.
[0016] In one embodiment, the tempering step includes placing the precursor glass in a mixed molten salt comprising 40-50% sodium nitrate and 50-60% potassium nitrate by mass, and keeping the mixture at 400-420° C. for 1-6 hours.
[0017] In one embodiment, before the tempering step, one or more steps of grinding, polishing and hot bending are also included.
[0018] In another aspect of the present invention, a cover glass is provided, comprising the lithium aluminosilicate glass.
[0019] By using the lithium aluminum silicate glass with the mass percentage of the components in the present invention, the Na-CS30 and Na-Dol high point areas last longer, which can effectively avoid attenuation during the tempering process, thereby preventing the glass from easily forming a large number of microcracks under the stress relaxation state, resulting in a decrease in the glass's sandpaper drop resistance. At the same time, it helps technicians to find the performance limit of the glass more quickly, reduce the time and economic cost of the exploration stage, and make the glass production and performance more stable. DETAILED DESCRIPTION
[0020] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0022] The following is a detailed description of a lithium aluminum silicate glass and a preparation method thereof provided in an embodiment of the present invention.
[0023] The present invention provides a lithium aluminum silicate glass, wherein the components of the lithium aluminum silicate glass include, by mass fraction, 48% to 68% SiO2, 16%≤Al2O3<23%, 2%≤Li2O<4%, 2% to 9% Na2O, 0.5% to 4% K2O, 1% to 6% MgO, 0 to 4% CaO, 3% to 8% B2O3, 0 to 2% P2O5, 0.1% to 4% ZrO2 and 0 to 3% ZnO. The lithium aluminum silicate glass with the mass percentage of the components in the present invention has a long duration of Na-CS30 and Na-Dol high point regions, which can effectively avoid attenuation during the tempering process, thereby avoiding a large number of microcracks that are easy to appear in the glass under stress relaxation, resulting in a decrease in the sandpaper drop resistance of the glass.
[0024] Silicon dioxide (SiO2) is the main component that forms silicon-oxygen tetrahedrons and connects to form the glass skeleton. SiO2 can improve the strength and chemical stability of glass, and can also improve the scratch resistance of glass and reduce the thermal expansion coefficient of glass. In the components of the lithium aluminum silicate glass, the mass fraction of SiO2 is 48% to 68%, and the mass fraction of SiO2 includes but is not limited to: 48%, 51%, 54%, 56%, 58%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67% or 68%, preferably 56% to 68%, and more preferably 60% to 65%. When SiO2<48%, the glass structure is relatively soft and the mechanical properties are poor; when SiO2>68%, there are too many glass structures, the difficulty of glass melting increases sharply, and the preparation is difficult.
[0025] Alumina (Al2O3) is easy to form tetrahedral coordination, and [AlO4] tetrahedral coordination can help build a tighter network with [SiO4] tetrahedrons, and is an important component of the glass network structure. [AlO4] tetrahedrons can also significantly enhance the ion exchange capacity of glass during chemical strengthening, and improve the chemical stability and elastic modulus of glass. The volume of the network space formed will vary depending on the content of Al2O3. In the components of the lithium aluminum silicate glass, the mass fraction of Al2O3 is 16%≤Al2O3<23%, including but not limited to 16%, 17%, 18%, 19%, 20%, 21% or 22%. When the Al2O3 content is low, less than 16%, the ion exchange channel is insufficient, resulting in limited ion exchange. When the Al2O3 content is high, exceeding 23%, the ion exchange rate is too fast, resulting in blockage of the ion exchange channel and limited ion exchange depth.
[0026] Lithium oxide (Li2O) is an ideal flux in glass components. + The polarization characteristics of Li can effectively reduce the high temperature viscosity at high temperature and improve the melting and forming properties of glass. + It is beneficial to the secondary chemical strengthening of glass and improves its strength. The present invention uses a mixed molten salt of NaNO3 and KNO3 in the strengthening process to + With Na in molten salt +Ion exchange can increase the depth of the compressive stress layer in a shorter time, making the glass have better mechanical impact resistance. In the components of the lithium aluminum silicate glass, the mass percentage of Li2O is 2% to 4%, including but not limited to 2%, 2.4%, 2.6%, 3%, 3.2%, 3.6% or 3.9%, preferably 2% to 3.9%. If its mass percentage is higher than 4%, the ion exchange capacity is too strong, and excessive ion exchange is completed in a short time, resulting in excessive central tensile stress, reduced glass stability, and easy damage. If its mass fraction is lower than 2%, the fluxing effect is poor, the glass viscosity is significantly increased, and it is difficult to melt.
[0027] Sodium oxide (Na2O) is another major fluxing agent, which can significantly reduce the melting temperature of glass. It is also an essential component for ion exchange in chemical strengthening. Ion exchange can significantly enhance the scratch resistance of glass. In the components of the lithium aluminum silicate glass, the mass percentage of Na2O is 2% to 9%, including but not limited to 2%, 2.8%, 3%, 3.6%, 4%, 5%, 6%, 7%, 8% or 9%, preferably 2% to 6%. When the content of Na2O is higher than 9%, it is easy to cause the Li-Na capacity to decrease and the Li-Na exchange deep stress to be too low. When the content of Na2O is lower than 2%, it is easy to cause the Li-Na exchange stress layer Na-Dol to be too low and the K-Na exchange stress K-CS to be too low.
[0028] Potassium oxide (K2O) can improve the melting performance of glass. In the components of the lithium aluminum silicate glass, its mass percentage is 0.5% to 4%, including but not limited to 0.5%, 1%, 1.8%, 2%, 2.5%, 3% or 4%, preferably 1% to 2.5%. If the content is higher than 4%, the K-Na exchange stress K-CS is too low, and if the content is lower than 0.5, the K-Na exchange stress K-Dol is too low.
[0029] Magnesium oxide (MgO) can reduce the viscosity of glass at high temperature, promote the melting and clarification of glass, enhance the stability of glass network space at low temperature, have a good repair effect on the gap of glass silicon oxygen-aluminum oxygen network structure, reduce the thermal expansion coefficient of glass to a certain extent, and increase the low temperature viscosity of glass, and improve the strain point and Young's modulus of glass. However, when the MgO content is too high, the surface tension of glass will be increased, making it difficult for alkali metal ions to exchange with glass, and there will be a certain hindering effect on ion exchange. Therefore, in the components of the lithium aluminum silicate glass, the mass fraction of MgO is 1% to 6%, including but not limited to 1%, 1.2%, 1.6%, 2%, 2.4%, 2.6%, 2.8%, 3%, 3.5%, 4%, 5% or 6%, preferably 1% to 4%. When the MgO content is higher than 6%, the K-Na and Li-Na exchanges are greatly hindered, the stress and stress depth of ion exchange are significantly reduced, and the improvement of mechanical properties is limited. When the MgO content is lower than 1%, the viscosity of the glass cannot be effectively reduced, resulting in excessively high viscosity of the glass, which is difficult to melt.
[0030] Calcium oxide (CaO) can lower the melting point of glass, improve the melting performance of glass at high temperature, and make the glass less likely to lose clarity. When the CaO content is too low, the melting point of the glass is high. When the CaO content is too high, the crystallization ability of the glass is significantly improved, and it is easy to crystallize and lose clarity. At the same time, it seriously hinders ion exchange. Therefore, in the components of the boroaluminosilicate glass, the mass percentage of CaO is 0% to 4%. Specifically, the mass percentage of CaO includes but is not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1%, 2%, 3% or 4%. Preferably, the mass percentage of CaO is 0.1% to 4%, and more preferably, the mass percentage of CaO is 0.1% to 3%.
[0031] Boron oxide (B2O3) is a good flux. The spatial end network formed by it can slide within a certain range. When the glass is under stress, the glass can obtain a larger deformation to buffer, thereby reducing the elastic modulus of the glass and reducing the generation of cracks. However, when the B2O3 content exceeds 8%, the volatilization amount is large during glass melting, the glass surface is severely stratified, and a material skin is formed, which eventually leads to a large number of defects such as glass tendons and crystallization during molding. When the B2O3 content is lower than 3%, the glass exhibits softer characteristics, the hardness of the glass decreases, and the scratch resistance decreases. Therefore, in the components of the lithium aluminum silicate glass, the mass percentage of B2O3 is 3% to 8%, including but not limited to 3.1%, 3.6%, 3.8%, 4.2%, 4.8%, 5%, 5.6%, 6%, 7% or 8%, preferably 3% to 5%, and more preferably 3% to 4.5%.
[0032] The addition of phosphorus pentoxide (P2O5) can expand the voids in the glass network, thereby significantly increasing the ion exchange capacity of the glass. More importantly, the addition of P2O5 can increase the strain point of the glass, alleviate the stress relaxation problem during the ion exchange process to a certain extent, and increase the surface compressive stress value of the glass after chemical strengthening. However, when the P2O5 content is too high, the thermal expansion coefficient of the glass increases significantly, the glass viscosity increases, and the surface compressive stress value decreases. In the components of the lithium aluminosilicate glass, the mass percentage of P2O5 is 0% to 2%, including but not limited to 0.1%, 0.5%, 1%, 1.5% or 2%, preferably 0.1% to 2%.
[0033] Zirconium oxide (ZrO2) can improve the chemical stability and ion exchange performance of glass, increase the surface hardness of glass, and increase the pressure required for glass to form cracks, thereby making the glass more resistant to scratches and falls. However, too much ZrO2 will significantly increase the melting temperature of glass, and at the same time will cause defects such as stones, and there is a tendency to devitrification, which is not conducive to molding and has an adverse effect on production. Therefore, in the components of the lithium aluminum silicate glass, the mass fraction of ZrO2 is 0.1% to 4%, including but not limited to 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%, preferably 0.1% to 3%.
[0034] Zinc oxide (ZnO) can significantly reduce the high temperature viscosity of glass and enhance the stability of the glass network space at low temperatures, but it also has a significant inhibitory effect on ion exchange. In the components of the lithium aluminum silicate glass, the mass fraction of ZnO is 0% to 3%, including but not limited to 0%, 1%, 2%, 3%, preferably 0.1% to 3%.
[0035] In the present invention, in order to further avoid the attenuation of Li-Na exchange stress (Na-CS30) and ion exchange depth (Na-Dol) of the glass during tempering, it is necessary to control the mass fraction ratio of (Li+Na+P+Al) / (Mg+Ca+Zn+B) to be less than 4. When (Li+Na+P+Al) / (Mg+Ca+Zn+B) is less than 4.0, the glass can continuously increase the strengthening stress depth Na-Dol during tempering, and when (Li+Na+P+Al) / (Mg+Ca+Zn+B) is greater than or equal to 4, after the glass passes through the Na-CS30 and Na-Dol increasing stages, the Na-CS30 and Na-Dol will be synchronously attenuated.
[0036] Another aspect of the present invention provides a method for preparing lithium aluminosilicate glass, comprising the following steps:
[0037] The raw materials are weighed according to the components, heated to 1600° C. to 1800° C., and kept warm for 6 h to 8 h to prepare a molten liquid; the molten liquid is molded, annealed, and cooled to prepare a precursor glass; the precursor glass is tempered to prepare the lithium aluminum silicate glass.
[0038] In one example, the annealing conditions include: annealing temperature is T, time is 2h to 4h, where T = T g +(30℃~50℃),T g is the glass transition temperature.
[0039] In one example, the glass transition temperature T g 10 is the viscosity fitting curve 13.4 P is the temperature corresponding to the viscosity.
[0040] In one example, the cooling step includes: cooling to the glass strain point temperature at a cooling rate of 1°C / min to 2°C / min, and then cooling to room temperature in the furnace.
[0041] In one example, the glass strain point temperature Tst is 10 14.5 P viscosity corresponding to the temperature
[0042] In one example, before the tempering step, one or more steps of grinding, polishing and hot bending are also included.
[0043] In one example, the tempering treatment step includes: placing the precursor glass in a mixed molten salt including 40% to 50% sodium nitrate and 50% to 60% potassium nitrate by mass, and keeping the temperature at 400° C. to 420° C. for 1 hour to 6 hours.
[0044] By using the lithium aluminum-silicon-aluminosilicate glass with the component mass percentage in the present invention, the Na-CS30 and Na-Dol high point areas last longer, which can effectively avoid attenuation during the tempering process, thereby preventing the glass from easily forming a large number of microcracks under stress relaxation, resulting in a decrease in the glass's anti-sandpaper drop performance.
[0045] Another aspect of the present invention provides a cover glass comprising the lithium aluminosilicate glass.
[0046] In the embodiment of the present invention, the stress (Na-CS30) and the exchange depth (Na-Dol) of lithium-sodium ion exchange of lithium aluminosilicate glass are tested by using a Japanese Orihara SLP2000 (365 nm) stress meter and referring to the standards GB / T18144-2008 and ASTM1422C-99.
[0047] It can be understood that the above-mentioned test methods and test equipment are commonly used methods for evaluating glass-related properties in the industry. They are only a means to characterize or evaluate the technical scheme and technical effects of the present invention. Other test methods and test equipment may also be used without affecting the final results.
[0048] The drop performance of the glass sandpaper in the embodiment of the present invention is tested by GP-2112 of a high-quality instrument, using a 180g steel block and 180-mesh sandpaper. Specifically, the drop starts from 0.4m. If the sample does not break, the drop depth is increased and continued until the sample breaks, and the breaking height is recorded.
[0049] The lithium aluminum silicate glass and the preparation method thereof provided by the present invention are described in detail below in conjunction with specific embodiments.
[0050] The following are specific embodiments.
[0051] Examples 1 to 21
[0052] Examples 1 to 21 all provide lithium aluminum silicate glass. According to the mass percentage of each component in Table 1, the raw materials corresponding to each component are calculated and weighed, and after being fully stirred and mixed, they are put into a platinum crucible, and then the platinum crucible is heated to 1650°C, melted and clarified for 6 hours, homogenized and cast into a glass brick with a size of 175mm×100mm, and then the glass brick is cast into a glass brick with a size of 175mm×100mm at T g + (30 ℃ ~ 50 ℃) temperature for 2 hours, and then cooled to the glass strain point temperature Tst at a cooling rate of 1 ℃ / min, and then taken out after cooling to room temperature in the furnace to obtain the precursor glass. The precursor glass is cut into a glass sheet with a thickness of 0.75mm by a precision wire cutting machine, and then the glass sheet is ground and polished to 0.6mm by a planetary grinding and polishing machine, and the glass surface is magnified without pitting. The polished glass is cut into 148.6mm × 68.4mm, and then processed into 2.5D cover glass by CNC and 2.5D scanning. The above cover glass is tempered by Suzhou Xinfut tempering furnace, and the temperature is calibrated by a contact thermometer. The tempering treatment specifically includes the following steps: the above cover glass is placed in a mixed molten salt containing 50% sodium nitrate and 50% potassium nitrate, and kept at 410℃ for 1 hour, 2 hours, 3 hours, 4 hours, 5 hours and 6 hours respectively to obtain lithium aluminum silicate glass. The stress of lithium sodium ion exchange (Na-CS30) and the depth of exchange (Na-Dol) of lithium aluminosilicate glass were tested.
[0053] Table 1 Composition (mass percentage)
[0054] Components Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 <![CDATA[SiO2]]> 48 49 50 52 53 57 57 <![CDATA[Al2O3]]> 22.8 22.5 22.5 22.85 20 18 22.5 <![CDATA[Li2O]]> 2.2 3.5 3.8 2.15 3.8 3.9 3.5 <![CDATA[Na2O]]> 9 6 4.2 5 2.7 3 3 <![CDATA[K2O]]> 1.5 2 2 2 4 3.5 2 MgO 2 2 5 3 4 2.5 2 CaO 4 2.5 2 3 3 2 2.5 <![CDATA[B2O3]]> 8 5 6.5 4.9 7 6 3 <![CDATA[ZrO2]]> 0.5 3.5 2 4 2 1.5 2 <![CDATA[P2O5]]> 2 2 1.5 1 0.1 1.6 1.5 ZnO 0 2 0.5 0.1 0.4 1 1 total 100 100 100 100 100 100 100 α 2.57 2.96 2.29 2.82 1.85 2.30 3.59
[0055] Note: α=(Li+Na+P+Al) / (Mg+Ca+Zn+B)
[0056]
[0057]
[0058]
[0059] The lithium aluminum silicate glasses prepared in Examples 1 to 21 were tested, and the test results are shown in Table 2.
[0060] Table 2 Lithium aluminum silicate glass performance test (unit: μm)
[0061]
[0062]
[0063]
[0064]
[0065] Comparative Examples 1 to 7
[0066] The preparation methods of Comparative Examples 1 to 7 are substantially the same as those of Examples 1 to 21, except that the mass percentages of the components are different, as shown in Table 3 below.
[0067] Table 3 Composition (mass percentage)
[0068]
[0069] The lithium aluminum silicate glasses prepared in Comparative Examples 1 to 7 were tested, and the test results are shown in Table 4.
[0070] Table 4 Lithium aluminum silicate glass performance test (unit: μm)
[0071]
[0072] A sandpaper drop test was performed on Examples 3, 13, 14 and Comparative Examples 5 and 6. The test results are shown in Table 5.
[0073] Table 5 Lithium aluminum silicate glass sandpaper drop test (unit: m)
[0074]
[0075]
[0076] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0077] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A lithium aluminosilicate glass, characterized in that: Measured by mass fraction, the components of the lithium aluminosilicate glass include: 48% to 68% SiO2, 16%≤Al2O3<23%, 2%≤Li2O<4%, 2% to 9% Na2O, 0.5% to 4% K2O, 1% to 6% MgO, 0 to 4% CaO, 3% to 8% B2O3, 0 to 2% P2O5, 0.1% to 4% ZrO2 and 0 to 3% ZnO; wherein, measured by mass fraction, (Li2O+Na2O+P2O5+Al2O3) / (MgO+CaO+ZnO+B2O3)<4.
2. The lithium aluminosilicate glass according to claim 1, characterized in that Measured by mass fraction, the components of the aluminosilicate glass include: 56% to 68% SiO2, 16% to 22% Al2O3, 2% to 3.9% Li2O, 2% to 6% Na2O, 1% to 2.5% K2O, 1% to 4% MgO, 0.1% to 4% CaO, 3% to 5% B2O3, 0.1% to 2% P2O5, 0.1% to 3% ZrO2 and 0.1% to 3% ZnO.
3. The lithium aluminosilicate glass according to claim 1, characterized in that Measured by mass fraction, the components of the aluminosilicate glass include: 60% to 65% SiO2, 17% to 21% Al2O3, 3% to 3.9% Li2O, 2% to 4% Na2O, 1% to 2% K2O, 2% to 4% MgO, 0.1% to 3% CaO, 3% to 4.5% B2O3, 0.5% to 2% P2O5, 0.1% to 2% ZrO2 and 0.5% to 3% ZnO.
4. A method for preparing the lithium aluminosilicate glass according to any one of claims 1 to 3, characterized in that: The steps include: Weigh the raw materials according to the components, heat to 1600° C. to 1800° C., and keep the temperature for 6 h to 8 h to prepare a molten liquid; forming, annealing and cooling the molten liquid to prepare a precursor glass; The precursor glass is tempered to prepare the lithium aluminum silicate glass.
5. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The annealing conditions include: annealing temperature is T, time is 2h~4h, where T=T g +(30℃~50℃),T g is the glass transition temperature.
6. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The cooling step comprises: cooling to the glass strain point temperature at a cooling rate of 1°C / min to 2°C / min, and then cooling to room temperature in the furnace.
7. The method for preparing lithium aluminosilicate glass according to claim 4, characterized in that: The tempering treatment step includes: placing the precursor glass in a mixed molten salt including 40-50% sodium nitrate and 50-60% potassium nitrate by mass fraction, and keeping the temperature at 400° C. to 420° C. for 1 hour to 6 hours.
8. The method for preparing lithium aluminosilicate glass according to any one of claims 4 to 7, characterized in that: Before the step of tempering, one or more steps of grinding, polishing and hot bending are also included.
9. A cover glass, characterized in that: The invention comprises the lithium aluminosilicate glass as claimed in any one of claims 1 to 3.
Citation Information
Patent Citations
Aluminosilicate glass and preparation method thereof
CN115490423A