A high-strength, high-toughness, high-thermal-conductivity, ablation-resistant ceramic gradient-modified C / C composite material and preparation method thereof

By directionally growing SiC nanowires in low-density C/C composites and designing the gradient distribution of ceramic components, the problems of oxidative ablation and insufficient thermal conductivity of ceramic-modified C/C composites at high temperatures are solved, achieving high strength and toughness. , modified C/C composite material with high thermal conductivity and ablation resistance, which improves the thermal protection performance of the aircraft.

CN116396091BActive Publication Date: 2024-10-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310361192.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

In extreme environments, the thermal protection system of ceramic-modified C/C composite materials of hypersonic aircraft suffers from oxidation and ablation at high temperatures and insufficient thermal conductivity, resulting in structural damage. It is difficult for existing technologies to effectively alleviate the damage of ceramic-modified C/C composite materials. Local overheating and thermal stress concentration problems at the service front end.

Method used

Through the normal pressure CVD process, SiC nanowires are directionally grown in low-density C/C composite materials, and combined with the gradient distribution design of ceramic components, a carbon fiber-SiC nanowire multi-scale preform and a ceramic gradient distribution structure are constructed to realize the formation of SiC nanowires. In-situ directional growth and gradient distribution of ceramic components improve the material's thermal conductivity and resistance to oxidation and ablation.

Benefits of technology

The overall directional growth and large-area in-situ growth array of SiC nanowires on the surface of carbon fiber are realized, which enhances the thermal conductivity and ablation resistance of the material, and alleviates the structural damage caused by local overheating and thermal stress during the ablation process. Improved the stability of C/C composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116396091B_ABST
    Figure CN116396091B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-toughness, high-thermal-conductivity, ablation-resistant ceramic gradient-modified C / C composite material and a preparation method. SiC nanowires grown in situ on carbon fibers are obtained in a low-density C / C composite material by a normal-pressure CVD process, and a carbon fiber-SiC nanowire multi-scale preform is constructed. And combined with the structural design of the gradient distribution of ceramic components and the subsequent densification process, a directional SiC nanowire and a synergistically modified C / C composite material with gradient distribution of ceramic components are finally prepared. The present invention adopts a catalyst-assisted gas-liquid-solid (VLS) mechanism, and the prepared SiC nanowires are obviously oriented overall on the surface of a single carbon fiber, and a large-area, repeatable in-situ directional growth array effect is achieved inside a low-density C / C. Compared with randomly oriented SiC nanowires, the in-situ directional growth of SiC nanowires and the matrix produces nanoscale mechanical interlocking, so that the load can be effectively transferred from the matrix to the nanowires, which is considered to have a more excellent toughening effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to a modified C / C composite material and a preparation method, and relates to a high-strength, high-thermal-conductivity, ablation-resistant ceramic gradient modified C / C composite material and a preparation method, and specifically relates to a method for constructing a high-strength, high-thermal-conductivity, ablation-resistant ceramic modified C / C composite material based on oriented SiC nanowires and ceramic gradient distribution. Background Art

[0002] When a hypersonic vehicle flies in the atmosphere at a speed several times that of Mach, the continuous high heat flux input causes the temperature of the thermal protection system such as the leading edge of the aircraft wing and the nose cone to rise rapidly. Once the service temperature of the thermal protection material is exceeded, the aircraft structure will be damaged or even disintegrated. Therefore, efficient thermal protection systems and thermal protection materials are the key foundation for the long-term and stable service of hypersonic vehicles in extreme environments. Carbon / carbon (C / C) composites have excellent comprehensive thermomechanical properties and have good application prospects in the field of ultra-high temperature thermal protection of advanced aircraft. However, the rapid oxidation and ablation of C / C composites in high-temperature oxygen environments is a major bottleneck that limits their further widespread application and development. At present, introducing anti-ablation ultra-high temperature ceramics (UHTCs) components into the C / C composite matrix is ​​an effective means to improve its anti-oxidation and ablation properties. However, UHTCs have the disadvantages of being brittle, having a high coefficient of thermal expansion, and the poor thermal conductivity of traditional ceramic-modified C / C composites. This causes aerodynamic heat to accumulate on the surface of the material when the aircraft is flying at ultra-high speed, high maneuverability, and long flight time, making it difficult to quickly transmit it to the rear, and generating a large temperature gradient and the resulting thermal stress that is stimulated and increases sharply, which can easily cause serious "stagnation point" ablation behavior and structural damage to the matrix. Therefore, how to alleviate the local overheating of the front end of the ceramic-modified C / C composite and simultaneously improve the structural stability of the matrix is ​​the key to further improving the long-term stable service of C / C-UHTCs composites.

[0003] In response to the serious heat accumulation at stagnation points in UHTCs thermal barrier coatings, which leads to increased thermal stress and the resulting cracking and peeling of the coating, researchers have proposed the idea of ​​constructing gradient coatings to alleviate thermal mismatch and regulate interface stress, which can effectively inhibit the generation of cracks in the coating (Paper 1 "Corrosion Science, 2022, 200:110215"); however, this method is mainly used in the field of coatings, and few people have studied the gradient modification scheme of C / C composite matrix. In addition, by introducing one-dimensional nanomaterials such as nanotubes and nanowires into the C / C preform to construct a nanomaterial-carbon fiber multi-scale preform, the carbon matrix can be effectively reinforced at the micro-nano scale, and the interface bonding between the fiber and the matrix can be improved, thereby improving the mechanical properties of the composite material (Reference 2 "Materials Science and Engineering: A, 2016, 651: 583-589"); in addition to improving the mechanical properties, studies have also shown that the introduction of SiC nanowires constructs a mesh interlocking structure, which can form a heat transfer channel inside the composite material and improve the thermal conductivity of the composite material (Reference 3 "Corrosion Science, 2016, 107: 9-20"); However, the SiC nanowires prepared by the existing process are randomly distributed and oriented inside the C / C matrix, which results in poor load and heat transfer effects, and the toughening and thermal conductivity improvement effects of the SiC nanowires are limited. Therefore, obtaining in-situ directional growth of SiC nanowires in the preform matrix and designing the gradient distribution of ceramic components are the key to further improving the thermal conductivity of modified C / C composites and synergistically improving their toughness and ablation resistance.

[0004] The present invention combines the gradient ceramic introduction technology with the atmospheric pressure CVD process to prepare the oriented SiC nanowire and the ceramic gradient distribution synergistic modified C / C composite material. The method obtains the oriented SiC nanowire-carbon fiber multi-scale mechanical interlocking structure and heat transfer channel in the carbon fiber preform, and effectively designs the ceramic gradient distribution modified carbon matrix, providing new technology and method for constructing high-strength, high-thermal conductivity, and ablation-resistant ceramic modified C / C composite materials. Summary of the invention

[0005] Technical issues to be solved

[0006] In order to avoid the shortcomings of the prior art, the present invention proposes a method for constructing ablation-resistant ceramic modified C / C composite materials based on oriented SiC nanowires and ceramic gradient distribution. It is a method for constructing high-strength, high-thermal-conductivity, and ablation-resistant ceramic modified C / C composite materials based on oriented SiC nanowires and ceramic gradient distribution. This scheme obtains SiC nanowires that are in-situ oriented and grown on carbon fibers in a low-density C / C composite material by a normal-pressure CVD method, and constructs a carbon fiber-SiC nanowire multi-scale preform. And combined with the structural design of the gradient distribution of ceramic components and the subsequent densification process, a C / C composite material modified by oriented SiC nanowires and gradient distribution of ceramic components is finally prepared. The SiC nanowires prepared by the present invention have obvious overall orientation on the surface of a single carbon fiber, and achieve the effect of large-area, repeatable in-situ oriented growth of SiC nanowire arrays inside the low-density C / C. Combining the construction of SiC nanowire-carbon fiber multiscale structure with the gradient modification design of the ceramic component of the C / C matrix, not only can the entire C / C matrix be strengthened and toughened at the micro-nano scale; but also a high-content ceramic component containing SiC nanowires is designed in the anti-ablation zone of the C / C service front end, which can effectively inhibit the formation of rapid oxidation channels and the cracking of the carbon matrix during oxidation or ablation; in addition, the introduction of oriented SiC nanowires constructs a nano-scale rapid heat transfer channel between carbon fibers, and the ceramic component in the C / C presents a gradient distribution (from the service front end to the back end, the ceramic content gradually decreases), which helps to improve the thermal conductivity of the C / C composite material and achieve its rapid heat dissipation during ablation. A method for constructing a high-strength, high-toughness, high-thermal-conductivity, and ablation-resistant ceramic-modified C / C composite material based on oriented SiC nanowires and a gradient distribution of ceramic components.

[0007] Technical Solution

[0008] A method for constructing ablation-resistant ceramic modified C / C composite material based on oriented SiC nanowires and ceramic gradient distribution, characterized by the following steps:

[0009] Step 1: Pre-treating the low-density C / C composite material;

[0010] Step 2, directional preparation of SiC nanowires in the low-density C / C composite material: soaking the low-density C / C composite material treated in step 1 in a metal salt catalyst ethanol solution, taking it out and drying it to obtain a low-density C / C composite material loaded with a catalyst;

[0011] A mixed powder of SiO2, Si and C is placed at the bottom of a graphite crucible, and a low-density C / C sample loaded with a catalyst is suspended above the powder in the crucible, and the graphite crucible is placed in a high-temperature reaction chamber of an atmosphere sintering furnace; then, under the protection of an argon atmosphere with a flow rate of 10 to 200 mL / min, the temperature is raised to 1200 to 1800°C at a rate of 5 to 10°C / min, and the temperature is kept for 0.5 to 10 hours, the power is turned off, and the mixture is naturally cooled to room temperature, and SiC nanowires are directionally prepared in the low-density C / C composite material;

[0012] Step 3, introducing ceramic components in gradient distribution: using a ceramic component partitioning process or a selected area introduction process, introducing ceramic components in gradient distribution into the SiC nanowire-low-density C / C composite material prepared in step 2, and then drying and curing;

[0013] Step 4, heat treatment: The heat treatment parameters are: heat treatment at 800-2500° C. for 1-10 h under the protection of 10-200 mL / min argon or nitrogen gas to transform or sinter the ceramic, and finally achieve a gradient distribution of ceramic components in the C / C matrix.

[0014] The pretreatment of the low-density C / C composite material in step 1 is performed by ultrasonic cleaning with anhydrous ethanol and deionized water for 10 to 70 minutes, and then placed in an oven at 60 to 100° C. for 5 to 24 hours until it is dried.

[0015] The density of the low-density C / C composite material is 0.45-1.2 g / cm 3 Low density C / C composite materials.

[0016] The concentration of the metal salt catalyst ethanol solution is 0.1-2 mol / L.

[0017] The step of soaking in the metal salt catalyst ethanol solution is 2 to 24 hours.

[0018] The mass percentage of the mixed powder of SiO2, Si and C is 1:0.1-0.6:0.2-0.8.

[0019] The metal salt catalyst ethanol solution includes, but is not limited to, ferric nitrate, cobalt nitrate, nickel nitrate, ferrous sulfate, cobalt sulfate, nickel sulfate, ferric chloride, cobalt chloride or nickel chloride.

[0020] The ceramic slurry includes but is not limited to: one or more of ZrB2, HfB2, TaB2, ZrC, HfC, TaC, SiC or MoSi2.

[0021] The ceramic component zoning process or selective introduction process includes but is not limited to: a combination of one or more of the following: polymer precursor zoning impregnation cracking method, ceramic slurry zoning impregnation method, ceramic slurry selective injection method, and ultrasonic zoning impregnation method, and is optimized in the impregnation depth process parameters and within the range of the components and content of the impregnation slurry.

[0022] A high-strength, high-thermal-conductivity, and ablation-resistant ceramic-modified C / C composite material based on oriented SiC nanowires and ceramic gradient distribution is characterized in that: SiC nanowires are integrally and repeatedly grown in situ on the surface of a single carbon fiber to form an SiC nanowire array; a high-content ceramic component containing SiC nanowires is present in the anti-ablation zone at the front end of the C / C service; the introduction of oriented SiC nanowires constructs a nanoscale heat transfer channel between the carbon fibers; the ceramic components in the C / C present a gradient distribution to improve the thermal conductivity of the C / C composite material during heat dissipation during ablation; the ceramic components in the C / C present a gradient distribution in that the ceramic content gradually decreases from the front end to the back end of the service.

[0023] Beneficial Effects

[0024] The present invention proposes a method for constructing a high-toughness, high-thermal-conductivity, and ablation-resistant ceramic-modified C / C composite material based on oriented SiC nanowires and a gradient distribution of ceramic components. SiC nanowires that are in-situ oriented and grown on carbon fibers are obtained in a low-density C / C composite material by a normal-pressure CVD process, and a carbon fiber-SiC nanowire multi-scale preform is constructed. And combined with the structural design of the gradient distribution of ceramic components and the subsequent densification process, a oriented SiC nanowire and a gradient distribution of ceramic components synergistically modified C / C composite material are finally prepared. The present invention adopts a catalyst-assisted gas-liquid-solid (VLS) mechanism, and the prepared SiC nanowires are obviously oriented overall on the surface of a single carbon fiber, and a large-area, repeatable in-situ oriented growth array effect is achieved inside the low-density C / C. Compared with randomly oriented SiC nanowires, the in-situ oriented growth of SiC nanowires produces nanoscale mechanical interlocking with the matrix, so that the load can be effectively transferred from the matrix to the nanowires, which is considered to have a more excellent toughening effect.

[0025] In addition, after the introduction of SiC nanowires, the SiC nanowires overlap each other between adjacent carbon fibers to construct a nanoscale rapid heat transfer channel, which greatly increases the thermal conductivity of the composite material in both the parallel and perpendicular directions of the fiber axis, and is believed to accelerate the heat diffusion during the ablation process. In addition, the material prepared by the present invention has strong structural and thermal stability. In view of the local overheating caused by the ablation process and the stress concentration caused by the size, shape and large temperature gradient of the component, the present invention effectively designs a solution for ceramic gradient modified C / C matrix to achieve effective matching of thermal expansion coefficients, thereby alleviating the structural damage caused by local overheating and thermal stress during the ablation process, and provides new technologies and methods for improving the anti-oxidation / ablation properties of C / C composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 : A preparation process flow chart of C / C composite materials modified by synergistic modification of oriented SiC nanowires and ceramic gradient distribution; the flow chart clearly shows the preparation process proposed by the present invention, which is mainly divided into 3 steps and is simple to operate.

[0027] Figure 2 : Schematic diagram of the structure of the oriented SiC nanowires and ceramic gradient distribution synergistically modified C / C composite material prepared by the present invention.

[0028] 1 and 2 are different types of ceramics, and 3 is SiC nanowires. This figure shows the idea of ​​combining the construction of SiC nanowire-carbon fiber multi-scale structure with the gradient modification design of ceramic components in the C / C matrix. The prepared SiC nanowires have obvious overall orientation on the surface of a single carbon fiber, and achieve the effect of large-area, repeatable in-situ growth of SiC nanowire arrays inside the C / C matrix. The high-content ceramic components containing SiC nanowires are mainly present in the anti-ablation area at the front end of the C / C service. DETAILED DESCRIPTION

[0029] The present invention will now be further described with reference to the embodiments and the accompanying drawings:

[0030] Embodiment 1:

[0031] 1. Low-density C / C composite material processing: density is 0.85g / cm 3 The low-density C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 30 minutes, then placed in an oven at 80°C for 12 hours, dried, and taken out.

[0032] 2. Preparation of oriented SiC nanowires in low-density C / C composite materials: Prepare a nickel nitrate ethanol solution with a concentration of 1 mol / L, place the low-density C / C composite material in step 1 in the solution and soak for 2 hours, take it out, dry it and set it aside. Ball-mill and mix SiO2, Si, and C powders with a mass percentage of 1:0.4:0.5 and dry them. Then weigh 5g of the above mixed powder and place it at the bottom of a graphite crucible, and hang the low-density C / C sample loaded with catalyst above the powder in the crucible, and place the graphite crucible in the high-temperature reaction chamber of the atmosphere sintering furnace; then, under the protection of an argon atmosphere (flow rate of 50 mL / min), heat it to 1500°C at a rate of 6°C / min, keep it warm for 1 hour, turn off the power, cool it naturally to room temperature, and take out the sample.

[0033] 3. Gradient introduction of ultra-high temperature ceramics:

[0034] The zirconium carbide organic precursor and polycarbosilane are dissolved in a certain amount of xylene at a mass percentage of 3:1, and the mixture is fully mixed by ultrasonic oscillation. Then, the SiC nanowire-low-density C / C composite material prepared in step 2 is suspended in the precursor solution for vacuum impregnation for 30 minutes, taken out, and dried. During the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4. Then, under the protection of a flowing argon atmosphere (flow rate of 50mL / min), the temperature is raised to 1800°C at a rate of 5°C / min, kept warm for 2h, the power is turned off, and the composite material is naturally cooled to room temperature. Repeat the impregnation and cracking cycle until the weight gain of the composite material is less than 8%. Subsequently, the mass percentage of the zirconium carbide organic precursor and polycarbosilane in the xylene solution is adjusted to 2:1, and the immersion depth of the composite material is changed to 1 / 2, and the cycle is repeated until the weight gain is less than 5%. The mass percentage of the zirconium carbide organic precursor and polycarbosilane is adjusted to 4:3, and the immersion depth is changed to 3 / 4, and the cycle is repeated until the weight gain of the composite material is less than 2%. Finally, a gradient distribution structure is obtained in the C / C matrix, in which the ZrC content gradually decreases and the SiC content gradually increases from the front end to the back end of the service.

[0035] Embodiment 2:

[0036] 1. Low-density C / C composite material processing: density is 0.65g / cm 3 The low-density C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 30 minutes, then placed in an oven at 80°C for 10 hours, dried, and taken out.

[0037] 2. Preparation of oriented SiC nanowires in low-density C / C composite materials: Prepare an ethanol solution of iron nitrate with a concentration of 0.8 mol / L, place the low-density C / C composite material in step 1 in the solution and soak for 2.5 hours, take it out, dry it and set it aside. Ball-mill and mix SiO2, Si, and C powders with a mass percentage of 1:0.4:0.5 and dry them. Then weigh 5g of the above mixed powder and place it at the bottom of a graphite crucible, and hang the low-density C / C sample loaded with catalyst above the powder in the crucible, and place the graphite crucible in the high-temperature reaction chamber of the atmosphere sintering furnace; then, under the protection of an argon atmosphere (flow rate of 100 mL / min), heat it to 1600°C at a rate of 5°C / min, keep it warm for 1 hour, turn off the power, cool it naturally to room temperature, and take out the sample.

[0038] 3. Gradient introduction of ultra-high temperature ceramics:

[0039] ZrC, SiC and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.67:0.3, and the slurry is prepared by ultrasonic oscillation for 30 minutes and magnetic stirring for 15 hours. Subsequently, the SiC nanowire-low-density C / C composite material prepared in step 2 is suspended in the ceramic slurry for vacuum impregnation for 30 minutes, taken out and dried. During the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4. Then, under the protection of a flowing argon atmosphere (flow rate of 100mL / min), the temperature is increased to 190°C at a heating rate of 5°C / min, kept warm for 3h, then heated to 900°C at a heating rate of 1°C / min, kept warm for 3h, turned off the power, and cooled naturally to room temperature. Repeat the impregnation and heat treatment cycle until the weight gain is less than 10%. The mass percentage of ZrC, SiC and phenolic resin in the ethanol solution is adjusted to 1:1:0.36, and the immersion depth of the composite material is changed to 1 / 2, and the cycle is repeated until the weight gain is less than 7%. The mass percentage of ZrC, SiC and phenolic resin was adjusted to 1:1.5:0.45, and the immersion depth of the composite material was changed to 3 / 4, and the cycle was repeated until the weight gain of the sample was less than 3%. Finally, a gradient distribution structure was obtained in the C / C matrix, in which the ZrC content gradually decreased from the front end to the back end of the service, while the SiC content gradually increased.

[0040] Embodiment 3:

[0041] 1. Low-density C / C composite material processing: density is 0.65g / cm 3 The C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 25 min, then placed in an oven at 70°C for 15 h, dried, and taken out.

[0042] 2. Preparation of oriented SiC nanowires in low-density C / C composite materials: Prepare a cobalt nitrate ethanol solution with a concentration of 0.8 mol / L, place the low-density C / C composite material in step 1 in the solution and soak for 3 hours, take it out, dry it and set it aside. Ball-mill and mix SiO2, Si, and C powders with a mass percentage of 1:0.4:0.5 and dry them. Then weigh 8g of the above mixed powder and place it at the bottom of a graphite crucible, and hang the low-density C / C sample loaded with catalyst above the powder in the crucible, and place the graphite crucible in the high-temperature reaction chamber of the atmosphere sintering furnace; then, under the protection of an argon atmosphere (flow rate of 80 mL / min), heat it to 1600°C at a rate of 5°C / min, keep it warm for 1 hour, turn off the power, cool it naturally to room temperature, and take out the sample.

[0043] 3. Gradient introduction of ultra-high temperature ceramics:

[0044] ZrC, SiC and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.6-2:0.2-0.5, and the slurry is prepared by ultrasonic oscillation for 30 minutes and magnetic stirring for 12 hours. Subsequently, a syringe with ceramic slurry (the diameter of the syringe needle is ~0.1mm) is vertically inserted into the SiC nanowire-low-density C / C composite prepared in step 2 for half-height injection, and then the injection depth is gradually reduced until the slurry overflows; at the same injection height, the horizontal outward spiral injection is performed, that is, first injecting into the center of the composite material, and then gradually injecting into the outer edge, and the distance between adjacent points is less than 5mm. In the process of reducing the injection depth, the mass percentages of ZrC, SiC and phenolic resin in the slurry are 1:0.67:0.3, 1:1:0.36 and 1:1.5:0.45, respectively. Then, under the protection of flowing argon atmosphere (flow rate of 80 mL / min), the temperature was raised to 180°C at a rate of 7°C / min, kept at this temperature for 2 hours, and then raised to 1050°C at a rate of 1°C / min, kept at this temperature for 2.5 hours, the power was turned off, and the mixture was naturally cooled to room temperature. Finally, a gradient distribution structure was obtained in the C / C matrix, in which the ZrC content gradually decreased from the front end to the back end of the service, while the SiC content gradually increased.

[0045] Embodiment 4:

[0046] 1. Low-density C / C composite material processing: density is 0.80g / cm 3 The C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 30 min, then placed in an oven at 70°C for 14 h, dried, and taken out.

[0047] 2. Preparation of oriented SiC nanowires in low-density C / C composite materials: Prepare a cobalt nitrate ethanol solution with a concentration of 0.5 mol / L, place the low-density C / C composite material in step 1 in the solution and soak for 3 hours, take it out, dry it and set it aside. Ball-mill and mix SiO2, Si, and C powders with a mass percentage of 1:0.4:0.5 and dry them. Then weigh 6g of the above mixed powder and place it at the bottom of a graphite crucible, and hang the low-density C / C sample loaded with catalyst above the powder in the crucible, and place the graphite crucible in the high-temperature reaction chamber of the atmosphere sintering furnace; then, under the protection of argon atmosphere (flow rate of 80 mL / min), heat it to 1500℃ at a rate of 5℃ / min, keep it warm for 2 hours, turn off the power, cool it naturally to room temperature, and take out the sample.

[0048] 3. Gradient introduction of ultra-high temperature ceramics:

[0049] ZrB2, SiC, and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.67:0.3, ultrasonically oscillated for 30 minutes, and ball-milled for 10 minutes to prepare a slurry. Subsequently, the SiC nanowire-low-density C / C composite prepared in step 2 is suspended in the ceramic slurry for ultrasonic impregnation for 30 minutes, taken out, and dried. During the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4. Then, under the protection of a flowing argon atmosphere (flow rate of 80 mL / min), the temperature is increased to 150°C at a rate of 7°C / min, kept warm for 2 hours, and then heated to 950°C at a rate of 2°C / min, kept warm for 3 hours, turned off the power, and cooled naturally to room temperature. Repeat the impregnation and heat treatment cycle until the weight gain is less than 10%. The mass percentages of ZrB2, SiC, and phenolic resin in the ethanol solution are adjusted to 1:1:0.36, and the immersion depth of the composite material is changed to 1 / 2, and the cycle is repeated until the weight gain is less than 7%. The mass percentage of ZrB2, SiC and phenolic resin was adjusted to 1:1.5:0.45, and the immersion depth of the composite material was changed to 3 / 4, and the cycle was repeated until the weight gain of the composite material was less than 3%. Finally, a gradient distribution structure was obtained in the C / C matrix, in which the ZrB2 content gradually decreased and the SiC content gradually increased from the front end to the back end of the service.

[0050] Embodiment 5:

[0051] 1. Low-density C / C composite material processing: density is 0.65g / cm 3 The C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 25 min, then placed in an oven at 80°C for 10 h, dried, and taken out.

[0052] 2. Preparation of oriented SiC nanowires in low-density C / C composite materials: Prepare an ethanol solution of iron nitrate with a concentration of 0.8 mol / L, place the low-density C / C composite material in step 1 in the solution and soak for 2.5 hours, take it out, dry it and set it aside. Ball-mill and mix SiO2, Si, and C powders with a mass percentage of 1:0.4:0.5 and dry them. Then weigh 5g of the above mixed powder and place it at the bottom of a graphite crucible, and hang the low-density C / C sample loaded with a catalyst above the powder in the crucible, and place the graphite crucible in the high-temperature reaction chamber of an atmosphere sintering furnace; then, under the protection of an argon atmosphere (flow rate of 100 mL / min), heat it to 1500°C at a rate of 5°C / min, keep it warm for 1.5 hours, turn off the power, cool it naturally to room temperature, and take out the sample.

[0053] 3. Gradient introduction of ultra-high temperature ceramics:

[0054] ZrC, SiC and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.6-2:0.2-0.5, and the slurry is prepared by ultrasonic oscillation for 35 minutes and magnetic stirring for 10 hours. Subsequently, a syringe with ceramic slurry (the diameter of the syringe needle is ~0.8mm) is vertically inserted into the SiC nanowire-low-density C / C composite prepared in step 2 to inject at 3 / 4 height, and then the injection depth is gradually reduced until the slurry overflows; at the same injection height, the injection is horizontally spirally injected outward, that is, first injected into the center of the composite material, and then gradually injected to the outer edge, and the distance between adjacent points is less than 5mm. In the process of reducing the injection depth, the mass percentages of ZrC, SiC and phenolic resin in the slurry are 1:1.5:0.42, 1:1:0.36 and 1:0.67:0.3, respectively. Then, under the protection of a flowing argon atmosphere (flow rate of 100 mL / min), the temperature was raised to 180°C at a rate of 5°C / min, kept warm for 2 hours, and then raised to 1050°C at a rate of 3°C / min, kept warm for 2.5 hours, turned off the power, and cooled naturally to room temperature. The obtained sample was suspended in a polycarbosilane xylene solution and ultrasonically impregnated for 30 minutes, and the immersion depth of the composite material was controlled to be 3 / 4 during the impregnation process. Then, under the protection of a flowing argon atmosphere (flow rate of 200 mL / min), the temperature was raised to 1300°C at a rate of 5°C / min, kept warm for 2 hours, turned off the power, and cooled naturally to room temperature. Repeat the ultrasonic impregnation and cracking cycle until the weight gain of the composite material is less than 1%. Finally, a gradient distribution structure with a gradually decreasing ZrC content and a gradually increasing SiC content from the front end to the back end of the service was obtained in the C / C matrix.

[0055] The present invention proposes a method for constructing a high-strength, high-thermal-conductivity, and ablation-resistant C / C composite material based on oriented SiC nanowires and ceramic gradient modification. The technical solution provided by the present invention prepares a modified C / C composite material with strong structural and thermal stability, and obtains an oriented SiC nanowire-carbon fiber multi-scale mechanical interlocking structure and heat transfer channel in a low-density C / C to address local overheating and stress concentration caused by component size, shape, and large temperature gradients, and effectively designs a ceramic gradient modified C / C matrix, providing new technology and methods for constructing a high-strength, high-thermal-conductivity, and ablation-resistant C / C composite material.

[0056] The technical solution of the present invention is not limited to the specific implementation methods listed above, and various changes can be made. That is, all other embodiments obtained according to the claims and description of the present invention application belong to the protection scope of the present invention.

Claims

1. A method for preparing a high-toughness, high-thermal-conductivity, ablation-resistant ceramic gradient-modified C / C composite material. Features Here are the steps: Step 1: Pre-treat the low-density C / C composite material: take the density of 0.45~1.2 g / cm 3 The low-density C / C composite material was ultrasonically cleaned with anhydrous ethanol and deionized water for 10-70 min, and then placed in an oven at 60-100°C for 5-24 h until it was dried; Step 2, directional preparation of SiC nanowires in the low-density C / C composite material: soaking the low-density C / C composite material treated in step 1 in a metal salt catalyst ethanol solution for 2 to 24 hours, then taking it out and drying it to obtain a low-density C / C composite material loaded with a catalyst; The mass percentage of SiO is 1:0.4:0.

5. 2 A mixed powder of Si and C is placed at the bottom of a graphite crucible, and a low-density C / C sample loaded with a catalyst is suspended above the powder in the crucible, and the graphite crucible is placed in a high-temperature reaction chamber of an atmosphere sintering furnace; then, under the protection of an argon atmosphere with a flow rate of 10-200 mL / min, the temperature is raised to 1500-1600°C at a rate of 5-10°C / min, and the temperature is kept for 0.5-10 h, the power is turned off, and the mixture is naturally cooled to room temperature, and SiC nanowires are directionally prepared in the low-density C / C composite material; Step 3: Introduction of ceramic component gradient distribution: The zirconium carbide organic precursor and polycarbosilane are dissolved in a certain amount of xylene in a mass percentage of 3:1, and fully oscillated by ultrasonic until completely mixed to obtain a precursor solution. Subsequently, the SiC nanowire-low-density C / C composite material prepared in step 2 is suspended in the precursor solution and vacuum impregnated for 30 minutes, taken out, and dried; During the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4, and then under the protection of a flowing argon atmosphere, the temperature is raised to 1800°C at a rate of 5°C / min, kept at this temperature for 2 h, the power is turned off, and the material is naturally cooled to room temperature. The impregnation and cracking cycle is repeated until the weight gain of the composite material is less than 8%. Subsequently, the mass percentage of zirconium carbide organic precursor and polycarbosilane in the xylene solution is adjusted to 2:1, and the immersion depth of the composite material is changed to 1 / 2, and the cycle is repeated until the weight gain is less than 5%. The mass percentage of zirconium carbide organic precursor and polycarbosilane is adjusted to 4:3, and the immersion depth is changed to 3 / 4, and the cycle is repeated until the weight gain of the composite material is less than 2%. Finally, a gradient distribution structure in which the ZrC content gradually decreases and the SiC content gradually increases from the service front end to the rear end is obtained in the C / C matrix; Alternatively, ZrC, SiC, and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.67:0.3, and a slurry is prepared by ultrasonic oscillation for 30 min and magnetic stirring for 15 h. Then, the SiC nanowire-low-density C / C composite material prepared in step 2 is suspended in the slurry for vacuum impregnation for 30 min, taken out, and dried; during the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4, and then, under the protection of a flowing argon atmosphere, the temperature is increased to 190°C at a heating rate of 5°C / min, and the temperature is kept for 3 h, and then the temperature is increased to 900°C at a heating rate of 1°C / min, and the temperature is kept for 3 h. h, turn off the power, cool naturally to room temperature, repeat the immersion and heat treatment cycle until the weight gain is less than 10%, adjust the mass percentage of ZrC, SiC and phenolic resin in the ethanol solution to 1:1:0.36, and change the immersion depth of the composite material to 1 / 2, repeat the cycle until the weight gain is less than 7%, adjust the mass percentage of ZrC, SiC and phenolic resin to 1:1.5:0.45, and change the immersion depth of the composite material to 3 / 4, repeat the cycle until the weight gain of the sample is less than 3%, and finally obtain a gradient distribution structure in which the ZrC content gradually decreases from the service front end to the rear end, while the SiC content gradually increases in the C / C matrix; Alternatively, ZrB 2 , SiC, and phenolic resin are mixed in a certain amount of ethanol solution in a mass percentage of 1:0.67:0.3, and a slurry is prepared by ultrasonic oscillation for 30 min and ball milling for 10 h. Subsequently, the SiC nanowire-low-density C / C composite material prepared in step 2 is suspended in the slurry for ultrasonic impregnation for 30 min, taken out, and dried; during the impregnation process, the immersion depth of the composite material is controlled to be 1 / 4, and then under the protection of a flowing argon atmosphere, the temperature is increased to 150°C at a rate of 7°C / min, and the temperature is kept for 2 h, and then the temperature is increased to 950°C at a rate of 2°C / min, and the temperature is kept for 3 h. The power is turned off and the mixture is naturally cooled to room temperature. The impregnation and heat treatment cycle is repeated until the weight gain is less than 10%, and the ZrB content in the ethanol solution is adjusted. 2 The mass percentage of SiC and phenolic resin was 1:1:0.36, and the immersion depth of the composite material was changed to 1 / 2, and the cycle was repeated until the weight gain was less than 7%. ZrB 2 The mass percentage of SiC and phenolic resin was 1:1.5:0.45, and the immersion depth of the composite material was changed to 3 / 4, and the cycle was repeated until the weight gain of the composite material was less than 3%, and finally a ZrB was obtained from the front end to the back end in the C / C matrix. 2 Gradient distribution structure in which the content of Si gradually decreases and the content of SiC gradually increases; Alternatively, ZrC, SiC, and phenolic resin are mixed in a certain amount of ethanol solution at a mass percentage of 1:0.6~2:0.2~0.5, and a slurry is prepared by ultrasonic oscillation for 35 min and magnetic stirring for 10 h. Subsequently, a syringe with ceramic slurry is vertically inserted into the SiC nanowire-low-density C / C composite prepared in step 2 to inject at a height of 3 / 4, and then the injection depth is gradually reduced until the slurry overflows; at the same time, the injection is horizontally spirally injected outward at the same injection height, that is, first inject into the center of the composite material, and then gradually inject to the outer edge, and the distance between adjacent points is less than 5 mm; in the process of reducing the injection depth, the mass percentages of ZrC, SiC, and phenolic resin in the slurry are 1:1.5:0.42, 1:1:0.36, and 1:0.67:0.3, respectively, and then, under the protection of a flowing argon atmosphere, the temperature is raised to 180°C at a heating rate of 5°C / min, and kept warm for 2 h, and then the temperature is raised to 1050°C at a heating rate of 3°C / min, and kept warm for 2.5 h, turn off the power, and cool naturally to room temperature; the obtained sample is suspended in a polycarbosilane xylene solution and ultrasonically impregnated for 30 min, and the immersion depth of the composite material is controlled to be 3 / 4 during the impregnation process, and then, under the protection of a flowing argon atmosphere, the temperature is increased to 1300°C at a rate of 5°C / min, and the temperature is kept for 2 h, and the power is turned off and naturally cooled to room temperature; the ultrasonic impregnation and cracking cycles are repeated until the weight gain of the composite material is less than 1%, and finally a gradient distribution structure is obtained in the C / C matrix, in which the ZrC content gradually decreases from the service front end to the back end, while the SiC content gradually increases; The metal salt in the metal salt catalyst ethanol solution includes: ferric nitrate, cobalt nitrate, nickel nitrate, ferrous sulfate, cobalt sulfate, nickel sulfate, ferric chloride, cobalt chloride or nickel chloride.

2. A modified C / C composite material prepared by the method for preparing a high-toughness, high-thermal-conductivity, ablation-resistant ceramic gradient modified C / C composite material according to claim 1, Features: SiC nanowires are integrally and repeatedly grown in situ on the surface of a single carbon fiber. A high-content ceramic component containing SiC nanowires is present in the anti-ablation zone at the service front end of the C / C composite material. The introduction of the oriented SiC nanowires constructs a nanoscale heat transfer channel between the carbon fibers. The ceramic components in the C / C composite material present a gradient distribution, which improves the thermal conductivity of the C / C composite material in the heat dissipation process. The ceramic components in the C / C composite material present a gradient distribution, and the ceramic content gradually decreases from the service front end to the rear end.