A method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy

Through the electromagnetic induction directional solidification phase separation method of Si-Ti-Cu alloy, the problems of uneven composition and low purity in the preparation of Cu3Si and Si-Ti alloys in the existing technology are solved, and alloy preparation of high purity and uniform composition is realized and simplified. improve the process and reduce costs.

CN116397120BActive Publication Date: 2024-10-22SICHUAN YONGAN LIGHT CYCLE PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310421938.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-22
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

It is difficult to prepare Cu3Si alloy and eutectic Si-Ti alloy with uniform composition and high purity at the same time using the existing technology, and the preparation process is complex, costly and difficult to control.

Method used

The electromagnetic induction directional solidification phase separation and purification method of Si-Ti-Cu alloy is used. According to the crystallization principle of the phase diagram, impurities segregate to prepare high-purity Cu3Si alloy and eutectic Si-Ti alloy with uniform structural composition.

Benefits of technology

It achieves the preparation of high-purity, uniform composition Cu3Si and Si-Ti alloys, reduces the impurity segregation coefficient, simplifies the process, avoids the generation of waste gas and waste residue, and is economical and sustainable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116397120B_ABST
    Figure CN116397120B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for simultaneously preparing a Cu3Si alloy and a eutectic Si-Ti alloy, and belongs to the technical field of alloy material preparation. The present invention uniformly mixes a Si material, a TiSi2 material and a metal copper material to obtain a mixed material, the mixed material is placed under vacuum or protective atmosphere conditions for induction heating and melting, and is smelted at a constant temperature for 2 to 3 hours to obtain a uniform Si-Ti-Cu alloy melt; under vacuum or protective atmosphere conditions, the Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain a Si-Ti-Cu alloy ingot, wherein the Si-Ti-Cu alloy ingot sequentially includes supermetallurgical grade Si or high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-enriched phase; the supermetallurgical grade Si or high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-enriched phase in the Si-Ti-Cu alloy ingot are cut along the phase interface to obtain supermetallurgical grade Si or high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-enriched phase, and the impurity-enriched phase is removed. The present invention can simultaneously prepare high-purity Cu3Si alloy and eutectic Si-Ti alloy with uniform organizational composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for simultaneously preparing a Cu3Si alloy and a eutectic Si-Ti alloy, belonging to the technical field of alloy material preparation. Background Art

[0002] Cu3Si alloy is a silicide with excellent performance. It is usually used as a catalyst in the production process of chlorosilane (raw material of silicone); in addition, Cu3Si can also be used to passivate copper-based chips, suppress diffusion and electron migration, and serve as a diffusion barrier. At present, Cu3Si is mainly prepared by vacuum sintering and mechanical alloying. However, the formability of Cu3Si alloy prepared by vacuum sintering is poor; and the purity of Cu3Si prepared by mechanical alloying cannot meet the standards for commercial use due to the contamination of ball milling media, and needs to be further purified.

[0003] Si-Ti eutectic alloy (composed of Si and TiSi2) is also a silicide material with excellent performance. It is widely used as a solder for SiC connection due to its good adhesion, wettability and high strength. At present, Si-Ti eutectic alloy is usually prepared by vacuum arc melting. However, when used as a solder for SiC connection, the Si-Ti eutectic alloy prepared by arc melting has the disadvantages of coarse phase structure and uneven composition, resulting in poor connection effect. Therefore, how to prepare a eutectic Si-Ti alloy with uniform composition is still difficult. In addition, Si-Ti eutectic alloy is also a very promising large-capacity lithium-ion battery material, and it is also required to have uniform composition when used as a large-capacity lithium-ion battery material.

[0004] The intermetallic compound TiSi2 has the characteristics of low density, high temperature oxidation resistance and high temperature strength, so it can be used as a high temperature structural material. In addition, since TiSi2 alloy also has low resistivity, TiSi2 plays an important role in integrated circuit contact and bonding technology, and is often used as gate wiring, interconnection line, Schottky diode and ohmic contact material. At present, TiSi2 alloys prepared by silicon reduction and molten salt electrolysis of titanium-containing slag cannot meet the purity requirements (>99.8%) of commercial TiSi2 alloys due to their low purity. At the same time, TiSi2, as an electronic material, will produce waste TiSi2 alloys with low purity as integrated circuits are scrapped.

[0005] At present, there is no clean and efficient method to prepare high-purity Cu3Si and eutectic Si-Ti alloys with uniform microstructure. Summary of the invention

[0006] The present invention aims at the problems of complex preparation process, low purity, high cost and difficult process control of existing Cu3Si alloy and eutectic Si-Ti alloy, and proposes a method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy. According to the crystallization principle of the phase diagram and the segregation of impurities, the present invention performs electromagnetic induction directional solidification phase separation and purification of Si-Ti-Cu alloy, and directly prepares high-purity Cu3Si alloy and eutectic Si-Ti alloy with uniform organizational composition.

[0007] A method for simultaneously preparing a Cu3Si alloy and a eutectic Si-Ti alloy, the specific steps are as follows:

[0008] (1) mixing Si material, TiSi2 material and metal copper material uniformly to obtain a mixed material, placing the mixed material under vacuum or protective atmosphere conditions for induction heating and melting, and smelting at a constant temperature for 2 to 3 hours to obtain a uniform Si-Ti-Cu alloy melt;

[0009] (2) Under vacuum or protective atmosphere conditions, the Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain a Si-Ti-Cu alloy ingot, wherein the Si-Ti-Cu alloy ingot sequentially comprises supermetallurgical grade Si or high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase;

[0010] Specifically, in the step (2), when the initial components in the Si-Ti-Cu alloy are located in the Si liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt includes supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence after directional solidification; when the initial components in the Si-Ti-Cu alloy are located in the TiSi2 liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt includes high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence after directional solidification;

[0011] (3) Supermetallurgical grade Si or high purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in Si-Ti-Cu alloy ingot are cut along the phase interface to obtain supermetallurgical grade Si or high purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase, and the impurity-rich phase is removed.

[0012] The TiSi2 material in step (1) is waste TiSi2 alloy, TiSi2 alloy prepared by silicon reduction of titanium-containing slag or TiSi2 alloy prepared by molten salt electrolysis, and the silicon material is waste solar cell silicon wafers, waste electronic silicon wafers, industrial silicon or silicon secondary resource recycling material.

[0013] In terms of mass percentage, the amount of metallic copper added to the mixed material in step (1) is 5-35%, the TiSi2 material accounts for 15-75%, and the Si material accounts for 10-80%.

[0014] The temperature of the electromagnetic induction directional solidification in step (2) is 1150-1350° C., and the moving speed of the directional solidification is no more than 1 μm / s.

[0015] The vacuum degree of the vacuum condition is not greater than 10Pa.

[0016] The principle of preparing Cu3Si alloy and eutectic Si-Ti alloy at the same time is as follows: the Si-Ti-Cu melt is separated according to the order of the crystallization temperatures of different crystals in the Si-Ti-Cu ternary system, that is, during the electromagnetic directional solidification process, Si (1414°C) or TiSi2 (1487°C) with a higher melting point is first precipitated at the bottom of the sample, and then the Si-Ti eutectic alloy (1330°C) is precipitated in the middle of the sample, and finally the Cu3Si alloy (851°C) with the lowest melting point is precipitated at the top of the sample, and finally a uniform, dense and high-purity alloy product is prepared to avoid the inclusion of other Si-Ti-Cu intermediate phases in the target alloy; in the Si-Ti-Cu melt When electromagnetic directional solidification is used to separate Si, the addition of Cu and Ti (TiSi2) refining agents reduces the crystallization temperature of Si, thereby reducing the segregation coefficient of impurities between solid Si and Si-Ti-Cu melt. In addition, since Ti has a strong affinity with boron and can form stable titanium boride, this further reduces the segregation coefficient of boron between solid silicon and Si-Cu-Ti melt, which allows more boron impurities to be continuously transferred from the solid to the liquid phase, thereby enhancing the purification of Si. When electromagnetic directional solidification is used to separate TiSi2 in a Si-Ti-Cu melt, the addition of Cu and Si refining agents also reduces the crystallization temperature of TiSi2. Similarly, this enhances the purification of TiSi2.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention performs directional solidification phase separation on Si-Ti-Cu melt according to the order of high and low crystallization temperatures of different crystals in the Si-Ti-Cu ternary system, and simultaneously prepares Cu3Si alloy and eutectic Si-Ti alloy with uniform microstructure, and obtains high-value supermetallurgical grade Si or high-purity TiSi2;

[0019] (2) The present invention reduces the segregation coefficient of impurities in Si / TiSi2 by adding a refining agent, thereby enhancing the removal effect of impurities and achieving efficient preparation of high-purity Cu3Si alloy and eutectic Si-Ti alloy;

[0020] (3) The present invention uses Cu as a refining agent, TiSi2 and Si as refining agents for each other, to prepare high-purity Cu3Si and eutectic Si-Ti alloys, thereby reducing the crystallization temperature of Si and TiSi2, strengthening the purification of Si and TiSi2, and achieving the sustainability of the preparation of Cu3Si alloys and eutectic Si-Ti alloys;

[0021] (4) The method of the present invention for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy does not generate waste gas, waste acid and waste residue, has a short flow, a simple process and is highly economical. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a process flow chart of the present invention;

[0023] Figure 2 The supermetallurgical grade silicon microstructure prepared in Example 1;

[0024] Figure 3 The microstructures of the eutectic Si-Ti alloy and Cu3Si alloy prepared in Example 1;

[0025] Figure 4 The microstructure of the high-purity TiSi2 alloy prepared in Example 2;

[0026] Figure 5 The microstructure of the eutectic Si-Ti alloy and Cu3Si alloy prepared in Example 2. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0028] Example 1: A method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy (see Figure 1 ), the specific steps are as follows:

[0029] (1) waste electronic silicon wafers (99.6%), waste TiSi2 (98.4%) and metal copper (99.5%) are uniformly mixed to obtain a mixed material (according to the crystallization liquid phase region of Si in the Si-Ti-Cu phase diagram, the mass ratio of the waste electronic silicon wafers, the waste TiSi2 alloy and the metal copper is 70:10:20), the mixed material is placed under a vacuum degree of 10 Pa for induction heating and melting, the heating temperature is 1350° C., and the mixed material is smelted at a constant temperature for 2 hours to fully volatilize the volatile impurities, so as to form a uniform Si-Ti-Cu alloy melt;

[0030] (2) Under the conditions of vacuum degree of 10 Pa and temperature of 1350°C, Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain Si-Ti-Cu alloy ingot, wherein the directional solidification movement rate is 1 μm / s. Since the initial components in the Si-Ti-Cu alloy are located in the Si liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt includes supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence after directional solidification;

[0031] (3) The supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in the Si-Ti-Cu alloy ingot were cut along the phase interface to obtain a supermetallurgical grade Si with a purity of 99.93wt% (see Figure 2 ), Si-Ti eutectic alloy with a purity of 99.1wt%, Cu3Si alloy with a purity of 99.0wt% (see Figure 3 ) and impurity-rich phase, the impurity-rich phase is removed.

[0032] Example 2: A method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy (see Figure 1 ), the specific steps are as follows:

[0033] (1) a TiSi2 alloy (97.2%) prepared by reducing titanium-containing slag with silicon, industrial silicon (99.3%) and metallic copper (99.5%) are uniformly mixed to obtain a mixed material (according to the crystallization liquid phase region of TiSi2 in the Si-Ti-Cu phase diagram, the mass ratio of the TiSi2 alloy prepared by reducing titanium-containing slag with silicon, industrial silicon and metallic copper is 55:18:27), the mixed material is induction heated and melted under argon atmosphere at a heating temperature of 1250° C., and is smelted at a constant temperature for 3 h to fully volatilize volatile impurities, thereby forming a uniform Si-Ti-Cu alloy melt;

[0034] (2) In an argon atmosphere and at a temperature of 1250°C, a Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain a Si-Ti-Cu alloy ingot, wherein the directional solidification movement rate is 0.5 μm / s. Since the initial components in the Si-Ti-Cu alloy are located in the TiSi2 liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt after directional solidification includes high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence;

[0035] (3) The high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in the Si-Ti-Cu alloy ingot were cut along the phase interface to obtain a high-purity TiSi2 with a purity of 99.83wt% (see Figure 4), Si-Ti eutectic alloy with a purity of 99.4wt%, Cu3Si alloy with a purity of 99.1wt% (see Figure 5 ) and impurity-rich phase, the impurity-rich phase is removed.

[0036] Example 3: A method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy (see Figure 1 ), the specific steps are as follows:

[0037] (1) TiSi2 alloy (97.7%) prepared by molten salt electrolysis, discarded solar cell silicon wafers (99.7%) and metallic copper (99.5%) are uniformly mixed to obtain a mixed material (according to the crystallization liquid phase region of TiSi2 in the Si-Ti-Cu phase diagram, the mass ratio of TiSi2 alloy prepared by molten salt electrolysis, discarded solar cell silicon wafers and metallic copper is 45:15:35), the mixed material is placed in a vacuum of 1 Pa for induction heating and melting, the heating temperature is 1150° C., and the mixed material is smelted at a constant temperature for 2.5 hours to fully volatilize volatile impurities, thereby forming a uniform Si-Ti-Cu alloy melt;

[0038] (2) Under the conditions of a vacuum degree of 1 Pa and a temperature of 1150°C, the Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain a Si-Ti-Cu alloy ingot, wherein the directional solidification movement rate is 0.1 μm / s. Since the initial components in the Si-Ti-Cu alloy are located in the TiSi2 liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt after directional solidification includes high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence;

[0039] (3) High-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in the Si-Ti-Cu alloy ingot are cut along the phase interface to obtain high-purity TiSi2 with a purity of 99.93wt%, Si-Ti eutectic alloy with a purity of 99.6wt%, Cu3Si alloy with a purity of 99.5wt% and impurity-rich phase, and the impurity-rich phase is removed.

[0040] Example 4: A method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy (see Figure 1 ), the specific steps are as follows:

[0041] (1) Industrial silicon (99.1%), TiSi2 alloy prepared by molten salt electrolysis (97.7%) and metallic copper (99.5%) are uniformly mixed to obtain a mixed material (according to the crystallization liquid phase region of Si in the Si-Ti-Cu phase diagram, the mass ratio of industrial silicon, TiSi2 alloy prepared by molten salt electrolysis and metallic copper is 65:10:25), the mixed material is placed in a vacuum degree of 0.1 Pa for induction heating and melting, the heating temperature is 1300°C, and the mixture is smelted at a constant temperature for 3 hours to fully volatilize the volatile impurities, so as to form a uniform Si-Ti-Cu alloy melt;

[0042] (2) Under the conditions of vacuum degree of 0.1 Pa and temperature of 1300°C, Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain Si-Ti-Cu alloy ingot, wherein the directional solidification movement rate is 1 μm / s. Since the initial components in the Si-Ti-Cu alloy are located in the Si liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt after directional solidification includes supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence;

[0043] (3) The supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in the Si-Ti-Cu alloy ingot are cut along the phase interface to obtain supermetallurgical grade Si with a purity of 99.95wt%, Si-Ti eutectic alloy with a purity of 99.1wt%, Cu3Si alloy with a purity of 99.1wt% and impurity-rich phase, and the impurity-rich phase is removed.

[0044] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for simultaneously preparing a Cu3Si alloy and a eutectic Si-Ti alloy, characterized in that: The specific steps are as follows: (1) mixing Si material, TiSi2 material and metal copper material uniformly to obtain a mixed material, placing the mixed material under vacuum or protective atmosphere conditions for induction heating and melting, and smelting at a constant temperature for 2 to 3 hours to obtain a uniform Si-Ti-Cu alloy melt; in terms of mass percentage, the amount of metal copper added to the mixed material is 5-35%, the TiSi2 material accounts for 15-75%, and the Si material accounts for 10-80%; (2) Under vacuum or protective atmosphere conditions, the Si-Ti-Cu alloy melt is subjected to electromagnetic induction directional solidification phase separation and purification to obtain a Si-Ti-Cu alloy ingot, wherein the Si-Ti-Cu alloy ingot sequentially comprises supermetallurgical grade Si or high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-enriched phase; the temperature of the electromagnetic induction directional solidification is 1150-1350° C., and the moving speed of the directional solidification is not greater than 1 μm / s; (3) Supermetallurgical grade Si or high purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in Si-Ti-Cu alloy ingot are cut along the phase interface to obtain supermetallurgical grade Si or high purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase, and the impurity-rich phase is removed.

2. The method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy according to claim 1, characterized in that: The TiSi2 material in step (1) is waste TiSi2 alloy, TiSi2 alloy prepared by silicon reduction of titanium-containing slag or TiSi2 alloy prepared by molten salt electrolysis, and the silicon material is waste solar cell silicon wafers, waste electronic silicon wafers, industrial silicon or silicon secondary resource recycling material.

3. The method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy according to claim 1, characterized in that: When the initial components in the Si-Ti-Cu alloy in step (2) are located in the Si liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt includes supermetallurgical grade Si, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence after directional solidification; when the initial components in the Si-Ti-Cu alloy are located in the TiSi2 liquid phase region of the Si-Ti-Cu ternary phase diagram, the Si-Ti-Cu melt includes high-purity TiSi2, Si-Ti eutectic alloy, Cu3Si alloy and impurity-rich phase in sequence after directional solidification.

4. The method for simultaneously preparing Cu3Si alloy and eutectic Si-Ti alloy according to claim 1, characterized in that: The vacuum degree of the vacuum condition is not greater than 10Pa.