Flame retardant fabric and preparation method thereof

By using melamine formaldehyde resin, isobornyl acrylate and sodium alginate, the preparation of flame retardant fabrics and combining alumina-graphene oxide composite materials, the existing flame retardant fabrics are solved inadequate fire resistance and water resistance in high temperature environments. Problem, high-strength, good flame retardant and heat insulation fabrics are suitable for protecting workers' lives and safety.

CN116397350BActive Publication Date: 2024-11-22JIHUA 3506 TEXTILE & APPL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310475911.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-22
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

The existing flame retardant fabrics are insufficient in high-temperature environments and cannot effectively protect the lives and safety of workers who are in high-temperature working environments for a long time.

Method used

The flame retardant fabric is prepared by melamine formaldehyde resin, isobornyl acrylate and sodium alginate. The composite fiber wire is generated by initiating reaction and wet spinning technology. The flame retardant fabric can be enhanced by alumina-graphene oxide composite material. and thermal insulation.

Benefits of technology

It improves the flame retardancy, strength and water resistance of the fabric, ensures good heat insulation and protection in high-temperature environments, and is suitable for long-term high-temperature working environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides a flame-retardant fabric and a preparation method thereof. The material of the flame-retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate. The oxygen-containing groups in the melamine formaldehyde resin are combined with the hydroxyl groups in the sodium alginate to improve the flame retardancy and breaking strength of the fiber; the isobornyl acrylate homopolymer has a high glass transition temperature and good heat resistance, and is polymerized with melamine formaldehyde resin and sodium alginate to improve the water washing resistance of spinning. The flame-retardant fabric of the present invention has a smooth surface and has high flame retardancy, strength and water washing resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant fabrics, and in particular to a flame retardant fabric and a preparation method thereof. Background Art

[0002] With the advancement of modern science and technology and the improvement of people's living standards, people have higher and higher functional requirements for clothing fabrics, especially for workers in firefighting, petrochemical, metallurgical casting, electric power and other industries who are in high-temperature working environments for a long time. Flame-retardant and fire-proof clothing is an important layer of skin related to life safety. This layer of "skin" not only isolates the human body from the fire source in a short period of time, but also replaces the human skin to accept the high temperature of the fire for a relatively long time. Therefore, flame-retardant and fire-proof clothing plays a vital protective role in the life safety of workers.

[0003] The invention patent with patent number CN112160155A discloses a flame retardant fabric, which uses vermiculite and polyvinyl alcohol to increase the fire resistance and flame retardancy of the fiber. Although the fabric is flame retardant, its strength is low and cannot meet the demand. Summary of the invention

[0004] In view of this, the present invention provides a flame retardant fabric with strong durability and water resistance and a preparation method thereof.

[0005] The technical solution of the present invention is implemented as follows: On the one hand, the present invention provides a flame retardant fabric, the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate.

[0006] The mass ratio of melamine formaldehyde resin: isobornyl acrylate: sodium alginate is (10-15): (3-5): (1-3).

[0007] In another aspect, the present invention provides a method for preparing a flame retardant fabric, comprising the following steps:

[0008] S1, adding melamine formaldehyde resin, isobornyl acrylate and an organic solvent into a reaction kettle, and then adding an initiator to initiate a reaction at 70-90° C.;

[0009] S2, after the initiation reaction is completed, sodium alginate is added, and the stirring reaction is continued for 2-3 hours, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0010] On the basis of the above technical solution, preferably, in the step S2, polyethylene glycol dimethyl ether and sodium alginate are added after the initiation reaction is completed, and the reaction is carried out at 70-90° C. for 2-3 hours.

[0011] On the basis of the above technical solution, preferably, the mass ratio of the polyethylene glycol dimethyl ether: melamine formaldehyde resin is (0.5-2): (10-15).

[0012] On the basis of the above technical solution, preferably, the organic solvent is one or more combinations of ethyl acetate, toluene, chloroform, acetone, dimethyl sulfoxide and N,N-dimethylformamide.

[0013] On the basis of the above technical solution, preferably, the mass ratio of the melamine formaldehyde resin: the organic solvent is (10-15): (50-80).

[0014] On the basis of the above technical solution, preferably, the initiator is an azo initiator or a peroxide initiator.

[0015] On the basis of the above technical solution, preferably, the mass ratio of the melamine formaldehyde resin:initiator is (10-15):(0.05-0.1).

[0016] On the basis of the above technical solution, preferably, the following step is further included: immersing the flame-retardant fabric prepared in step S2 in an aluminum oxide-graphene oxide composite material for 6-8 hours, washing and drying, to obtain a flame-retardant and heat-insulating fabric.

[0017] On the basis of the above technical scheme, preferably, the preparation method of the aluminum oxide-graphene oxide composite material is: ultrasonically disperse graphene oxide in deionized water, then add ammonium carbonate, stir evenly and adjust the pH of the mixed solution to 8-10, and then add aluminum phosphate aqueous solution under stirring conditions to obtain the aluminum oxide-graphene oxide composite material.

[0018] On the basis of the above technical solution, preferably, the mass ratio of graphene oxide to ammonium carbonate is (0.1-0.5) to (10-15).

[0019] The flame retardant fabric and preparation method of the present invention have the following beneficial effects compared with the prior art:

[0020] The flame-retardant fabric of the present invention has a smooth surface, high flame retardancy, strength, and good water resistance. Among them, melamine formaldehyde resin has low thermal conductivity, high nitrogen content, and good heat resistance. At the same time, the oxygen-containing groups in the melamine formaldehyde resin are combined with the hydroxyl groups in the sodium alginate to improve the flame retardancy and breaking strength of the fiber. Isobornyl acrylate homopolymer has a high glass transition temperature and good heat resistance. It is introduced into the fiber to improve the flame retardancy of the fiber. Melamine formaldehyde resin, sodium alginate and isobornyl acrylate generate composite fibers with high flame retardancy, strength and water washability.

[0021] Polyethylene glycol dimethyl ether is a flexible molecule that is easy to crystallize during polymerization. The crystalline part will play a role of physical cross-linking, thereby improving the strength and flexibility of the fiber.

[0022] Alumina-graphene oxide composite materials have a high specific surface area and abundant surface functional groups, which can be firmly adsorbed on the fiber surface to improve the flame retardancy and high temperature insulation properties of the fiber. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0026] S1, add 100g of melamine formaldehyde resin, 30g of isobornyl acrylate and 500g of ethyl acetate into a reactor, then add 0.5g of azobisisobutyronitrile, and initiate the reaction at 70°C for 1h;

[0027] S2, after the initiation reaction is completed, 10g of sodium alginate is added, and the reaction is continued with stirring at 70°C for 2h, and then wet spinning is performed to obtain composite fiber yarns. The composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0028] Example 2

[0029] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0030] S1, add 110g of melamine formaldehyde resin, 35g of isobornyl acrylate and 550g of dimethyl sulfoxide into a reaction kettle, then add 0.6g of azobisisoheptyl cyanide, and initiate the reaction at 75°C for 1h;

[0031] S2, after the reaction is completed, 15g of sodium alginate is added, and the reaction is continued with stirring at 75°C for 2.5h, and then wet spinning is performed to obtain composite fiber yarns. The composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0032] Example 3

[0033] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0034] S1, add 150g of melamine formaldehyde resin, 50g of isobornyl acrylate and 800g of N,N-dimethylformamide into a reactor, then add 1g of dibenzoyl peroxide, and initiate the reaction at 90°C for 1h;

[0035] S2, after the initiation reaction is completed, 30g of sodium alginate is added, and the reaction is continued with stirring at 90°C for 3h, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0036] Example 4

[0037] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate, polyethylene glycol dimethyl ether and sodium alginate; the fabric is prepared in the following steps:

[0038] S1, add 100g of melamine formaldehyde resin, 30g of isobornyl acrylate and 500g of ethyl acetate into a reactor, then add 0.5g of azobisisobutyronitrile, and initiate the reaction at 70°C for 1h;

[0039] S2, after the initiation reaction is completed, 15g of polyethylene glycol dimethyl ether and 10g of sodium alginate are added, and the reaction is continued at 70°C with stirring for 2h, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0040] Example 5

[0041] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate, polyethylene glycol dimethyl ether and sodium alginate; the fabric is prepared in the following steps:

[0042] S1, add 140g of melamine formaldehyde resin, 45g of isobornyl acrylate, 200g of ethyl acetate and 500g of acetone into a reactor, then add 0.8g of initiator azobisisobutyronitrile, and initiate the reaction at 86°C for 1h;

[0043] S2, after the initiation reaction is completed, 18g of polyethylene glycol dimethyl ether and 18g of sodium alginate are added, and the stirring reaction is continued at 90°C for 3h, and then wet spinning is performed to obtain composite fiber yarns. The composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics.

[0044] Example 6

[0045] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0046] S1, add 100g of melamine formaldehyde resin, 30g of isobornyl acrylate and 500g of ethyl acetate into a reactor, then add 0.5g of azobisisobutyronitrile, and initiate the reaction at 70°C for 1h;

[0047] S2, after the initiation reaction is completed, 15g of polyethylene glycol dimethyl ether and 10g of sodium alginate are added, and the reaction is continued at 70°C with stirring for 2h, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics;

[0048] S3, prepare an aluminum oxide-graphene oxide composite material: ultrasonically disperse 0.1 g of graphene oxide in 100 mL of deionized water, then add 0.2 g of ammonium carbonate, stir evenly and adjust the pH of the mixed solution to 8, and then add 500 mL of an aluminum phosphate aqueous solution with a mass concentration of 10% under stirring to obtain an aluminum oxide-graphene oxide composite material; immerse the flame-retardant fabric obtained in step S2 in the aluminum oxide-graphene oxide composite material for 6 hours, wash and dry, and obtain a flame-retardant and heat-insulating fabric.

[0049] Example 7

[0050] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0051] S1, add 145g of melamine formaldehyde resin, 48g of isobornyl acrylate, 300g of toluene and 350g of N,N-dimethylformamide into a reactor, then add 0.65g of azobisisoheptyl cyanide, and initiate the reaction at 90°C for 1h;

[0052] S2, after the initiation reaction is completed, 18g of polyethylene glycol dimethyl ether and 26g of sodium alginate are added, and the reaction is continued at 90°C with stirring for 3h, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics;

[0053] S3, a preparation method for an aluminum oxide-graphene oxide composite material is as follows: ultrasonically disperse 0.5 g of graphene oxide in 100 ml of deionized water, then add 0.5 g of ammonium carbonate, stir evenly and adjust the pH of the mixed solution to 10, and then add 500 mL of an aluminum phosphate aqueous solution with a mass concentration of 15% under stirring to obtain an aluminum oxide-graphene oxide composite material; immerse the flame-retardant fabric obtained in step S2 in the aluminum oxide-graphene oxide composite material for 8 hours, wash and dry, and obtain a flame-retardant and heat-insulating fabric.

[0054] Example 8

[0055] A flame retardant fabric, wherein the material of the flame retardant fabric yarn includes melamine formaldehyde resin, isobornyl acrylate and sodium alginate; the fabric is prepared in the following steps:

[0056] S1, add 146g of melamine formaldehyde resin, 48g of isobornyl acrylate and 750g of N,N-dimethylformamide into a reaction kettle, then add 0.85g of azobisisoheptyl cyanide, and initiate the reaction at 90°C for 1h;

[0057] S2, after the initiation reaction is completed, 20g of polyethylene glycol dimethyl ether and 28g of sodium alginate are added, and the reaction is continued at 90°C with stirring for 3h, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics;

[0058] S3, the preparation method of the aluminum oxide-graphene oxide composite material is: ultrasonically disperse 0.35g of graphene oxide in 100ml of deionized water, then add 0.25 ammonium carbonate, stir evenly and adjust the pH of the mixed solution to 9, and then add 500ml of an aluminum phosphate aqueous solution with a mass concentration of 13% under stirring to obtain the aluminum oxide-graphene oxide composite material; immerse the flame-retardant fabric obtained in step S2 in the aluminum oxide-graphene oxide composite material for 7h, wash and dry, and obtain a flame-retardant and heat-insulating fabric.

[0059] Comparative Example 1

[0060] The difference between Comparative Example 1 and Example 1 is the lack of melamine formaldehyde resin.

[0061] Comparative Example 2

[0062] The difference between Comparative Example 2 and Example 1 is the lack of isobornyl acrylate.

[0063] Comparative Example 3

[0064] The difference between Comparative Example 3 and Example 1 is that the content of isobornyl acrylate is 100 g.

[0065] Comparative Example 4

[0066] The difference between Comparative Example 4 and Example 4 is that the content of polyethylene glycol dimethyl ether is 50 g.

[0067] The composite fiber yarns are used as warp and weft yarns, with a linear density of 40 yarns / cm and a weft density of 30 yarns / cm, and are woven into flame-retardant fabrics using a weaving machine in a 2 / 2 twill weave.

[0068] The flame retardancy, strength and thermal insulation of the fabric were tested. The flame retardancy was measured by the limiting oxygen index (LOI) of the fabric according to GB / T 5454-1997. The washability was measured by washing the flame retardant fabric according to GB / T 17596-1988, and then measuring the properties of the washed fabric. The tear strength was the average value of the radial and dimensional directions. The results are as follows:

[0069] Table 1 Comparison of properties of fabrics of the embodiment and comparative example

[0070]

[0071] As shown in Table 1, the flame retardancy of the fabric prepared by the present invention reaches more than 35%, and the breaking strength reaches 6.7 cN.dtex -1 Above. Thermal protection is higher than 689KW.S / cm 2 , the tear strength is higher than 115N, and there is no melting dripping. After adding polyethylene glycol dimethyl ether to Example 4-5, the flame retardancy and strength are improved; after the fabric of Example 6-8 is impregnated with alumina-graphene oxide composite materials, the thermal protection and strength of the fabric are improved. This is because during polymerization, the crystalline part of polyethylene glycol dimethyl ether plays a role of physical cross-linking, thereby improving the strength and flame retardancy of the fiber; the large specific surface area and rich functional groups of the alumina-graphene oxide composite material are firmly adsorbed on the fiber surface, improving the thermal insulation and flame retardancy of the fiber.

[0072] Table 2 Comparison of washability of fabrics in the embodiment and comparative example (washed 50 times)

[0073]

[0074] It can be seen from Table 2 that the fabric of this embodiment has strong water washing resistance. After washing 50 times, it still has high flame retardancy and heat protection, while also maintaining high strength, and can be used for workers who are in a high temperature working environment for a long time.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a flame retardant fabric, characterized in that: The steps include: S1, adding melamine formaldehyde resin, isobornyl acrylate and an organic solvent into a reaction kettle, and then adding an initiator to initiate a reaction at 70-90° C.; S2, after the initiation reaction is completed, sodium alginate is added, the reaction is continued with stirring for 2-3 hours, and then wet spinning is performed to obtain composite fiber yarns, and the composite fiber yarns are interwoven and woven to obtain flame-retardant fabrics; In the step S2, after the initiation reaction is completed, polyethylene glycol dimethyl ether and sodium alginate are added and reacted at 70-90° C. for 2-3 hours; The mass ratio of the melamine formaldehyde resin: isobornyl acrylate: sodium alginate is (10-15): (3-5): (1-3); The mass ratio of the polyethylene glycol dimethyl ether to the melamine formaldehyde resin is (0.5-2): (10-15).

2. The method for preparing a flame retardant fabric according to claim 1, characterized in that: The organic solvent is one or more combinations of ethyl acetate, toluene, chloroform, acetone, dimethyl sulfoxide and N,N-dimethylformamide; the mass ratio of the melamine formaldehyde resin to the organic solvent is (10-15): (50-80).

3. The method for preparing a flame retardant fabric according to claim 1, characterized in that: The initiator is an azo initiator or a peroxide initiator; the mass ratio of the melamine formaldehyde resin to the initiator is (10-15) to (0.05-0.1).

4. The method for preparing a flame retardant fabric according to claim 1, characterized in that: The method also includes the following steps: immersing the flame-retardant fabric prepared in step S2 in an aluminum oxide-graphene oxide composite material for 6-8 hours, washing and drying, and obtaining a flame-retardant and heat-insulating fabric.

5. The method for preparing a flame retardant fabric according to claim 4, characterized in that: The preparation method of the aluminum oxide-graphene oxide composite material is: ultrasonically dispersing graphene oxide in deionized water, then adding ammonium carbonate, stirring evenly and adjusting the pH of the mixed solution to 8-10, and then adding an aluminum phosphate aqueous solution under stirring conditions to obtain the aluminum oxide-graphene oxide composite material.

6. The method for preparing a flame retardant fabric according to claim 5, characterized in that: The mass ratio of graphene oxide to ammonium carbonate is (0.1-0.5) to (10-15).