A molding method for ultra-microporous zinc-based MOF material
By using a variety of adhesives with different thermal decomposition temperatures and agitated extrusion molding techniques, the problem of adhesive blocking the pores is solved, and the mechanical strength and adsorption selectivity of ultra-microporous MOF materials are improved, which is suitable for industrial production. .
Patent Information
- Application Number
- CN202111681334.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-12-31
AI Technical Summary
In the existing ultramicroporous MOF material molding method, the adhesive easily blocks the pores, resulting in a degradation of material adsorption performance. The traditional method operates in a complicated manner, making it difficult to achieve high mechanical strength and selectivity improvement.
Use more than two binders with different thermal decomposition temperatures to mix, stir and extrude through deionized water, and then heat and activate in air or inert atmosphere to remove binders with lower thermal decomposition temperatures to retain high thermal decomposition The binder at temperature forms a molding agent with high mechanical strength.
The high mechanical strength and adsorption selectivity of the molding agent are achieved, avoiding the problem of adhesive blocking the holes, and simplifying the process operation, which is suitable for large-scale industrial applications.
Smart Images

Figure CN116408052B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the molding of MOF materials, and in particular to a molding method of ultra-microporous zinc-based MOF materials. Background Art
[0002] Ethylene is the core of the petrochemical industry, with an annual global output of over 100 million tons, and its products account for more than 70% of petrochemical products. In the process of ethylene production, ethane is often separated by low-temperature distillation to achieve purification, resulting in huge energy consumption. Adsorption separation technology has the characteristics of energy saving and high efficiency, and has received widespread attention from researchers in recent years. Metal-organic framework materials (MOFs) have regular pore structures and adjustable pore sizes, making them ideal gas separation materials. In recent years, MOF materials have also made many advances in the field of ethylene / ethane adsorption separation. Since the synthesized MOF materials are mostly in crystalline or powder state, they are brittle and easily broken into smaller particles or powders, making them difficult to directly apply in industrial processes. Therefore, molding is the only way for MOF materials to move towards industrial applications.
[0003] There are many methods for forming MOF powders. In addition to the traditional high-pressure granulation method, adhesive molding method, and in-situ growth method, there are also new processing methods such as freeze-drying, electrospinning, and hot pressing. Among the above-mentioned molding methods, the emerging methods are still in the laboratory stage, with high technical content and high difficulty in operation; the traditional methods are easy to operate, such as extrusion molding and ball molding, which have long been widely used in industry. However, since the strength of MOF materials is far inferior to that of traditional porous materials, high-pressure granulation can easily cause pore collapse, and the addition of adhesives will block the pores, resulting in a decrease in the adsorption performance of the material.
[0004] CN103586011A discloses a sintering-free molding coating method for ultra-high specific surface area metal organic framework material MIL-101, comprising the following steps: 1) MIL-101 powder material and binder are mixed in a certain proportion, and molded particles are obtained after kneading and extrusion, and the mass percentage of MIL-101 powder material in the molded particles is 40% to 98%; 2) the above molded particles are dried at 20°C to 180°C to obtain dried molded particles; 3) the dried molded particles are immersed in a polyvinyl alcohol solution with a mass concentration of 1% to 30%, immersed for 2 to 6 seconds, and after being completely coated with a polyvinyl alcohol film, dried at 20°C to 180°C to obtain molded coated particles. This method mixes the MOF material with an inorganic binder and then immerses it in a polyvinyl alcohol solution, so that the surface of the molding agent is coated with a polyethylene film, and the molding agent particles are obtained after drying. Although this method uses two adhesives, the aluminum-based adhesive needs to enter the pores and interact with the material to form bonds in order to achieve the purpose of bonding and molding, and is not suitable for ultra-microporous MOF materials.
[0005] CN110639475A discloses a method for mass synthesis and molding of UTSA-280 adsorbent materials, and particularly relates to a method for mass preparation of UTSA-280 MOFs materials by adjusting the reaction raw materials and the regulator, and using additives to mold and granulate the materials. 3 ·H 2 O promotes the dissolution of squaric acid, adds calcium nitrate aqueous solution to the formed squaric acid aqueous solution, keeps stirring during the addition of calcium nitrate aqueous solution, and obtains high crystallinity strip UTSA-280 crystals at room temperature. This molding method adds ethyl acetate solution of polymethyl methacrylate to UTSA-280 crystals, mixes and stirs, and then forms and granulates. The binder may cause pore blocking, which affects the separation performance of the material. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for forming an ultra-microporous MOF material. The obtained ultra-microporous MOF material not only has higher mechanical strength but also has improved adsorption selectivity.
[0007] To achieve the above object, the present invention provides a method for forming an ultra-microporous zinc-based MOF material, comprising the following steps:
[0008] (1) two or more binders with different thermal decomposition temperatures are stirred and mixed to form a composite binder; (2) the dried MOF material is mixed with the composite binder; (3) deionized water is added to the mixture of step (2) and mixed and stirred to obtain a paste, which is extruded to obtain a molding agent; (4) the molding agent is activated by heating in air, an inert atmosphere or vacuum conditions to remove part of the binder in the molding agent to obtain an activated molding agent.
[0009] In the molding method of the ultra-microporous zinc-based MOF material described in the present invention, preferably, the mass ratio of the composite binder to the MOF material is (0.05-0.2):1.
[0010] In the molding method of the ultra-microporous zinc-based MOF material of the present invention, it is preferred that the thermal decomposition temperatures of various binders in the composite binder differ by more than 50°C.
[0011] The molding method of the ultra-microporous zinc-based MOF material described in the present invention, wherein preferably, the composite binder includes a first binder and a second binder, and the thermal decomposition index of the first binder is higher than that of the second binder by more than 50°C; further preferably, the first binder is selected from at least one of pseudo-boehmite, silica sol, polyvinyl pyrrolidone, methyl cellulose, and polymethyl methacrylate; the second binder is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose, soluble starch, sucrose, glucose, and sodium alginate. The thermal decomposition temperatures of the binders selected in the present invention are shown in the following table:
[0012] Table 1 Binder thermal decomposition temperature table
[0013] name Thermal decomposition temperature (℃) Pseudoboehmite >350 Silica Sol >350 Polyvinylpyrrolidone 350 Methylcellulose 300 Polymethyl methacrylate 300 Polyvinyl alcohol 250 Carboxymethyl cellulose 250 Soluble starch 250 sucrose 220 glucose 220 Sodium alginate 230
[0014] In the molding method of the ultra-microporous zinc-based MOF material described in the present invention, it is preferred that the mass ratio of the first binder to the second binder is (0-1):1, and does not include 0.
[0015] In the method for forming the ultra-microporous zinc-based MOF material of the present invention, it is preferred that in step (3), the amount of deionized water added is 20 to 40 wt % of the mass of the mixture, and more preferably 20 to 25 wt %.
[0016] In the molding method of the ultra-microporous zinc-based MOF material of the present invention, it is preferred that the extrusion pressure of the extrusion molding is 70 to 250 kgf, and more preferably 90 to 120 kgf.
[0017] The molding method of the ultra-microporous zinc-based MOF material of the present invention is preferably that the ultra-microporous zinc-based MOF material is cylindrical with a diameter of 2 to 4 mm and a length of 2 to 5 mm.
[0018] The molding method of the ultra-microporous zinc-based MOF material of the present invention is preferably that the activation condition is: calcination in an inert nitrogen atmosphere at 200-350°C, and the temperature is more preferably 220-300°C.
[0019] The molding method of the ultra-microporous zinc-based MOF material of the present invention is preferably such that the thermal decomposition temperature of the ultra-microporous zinc-based MOF material is 300-500°C, and more preferably 370°C-420°C.
[0020] The molding method of the ultra-microporous zinc-based MOF material provided by the present invention has the following advantages:
[0021] (1) The activated molding agent obtained not only has high mechanical strength, but also solves the problem of reduced material adsorption and poor selectivity caused by pore blockage by the binder.
[0022] (2) Since the composite binder is composed of two or more binders with different thermal decomposition temperatures, the binder with a lower thermal decomposition temperature can be removed in a controllable manner by controlling the calcination temperature, while the binder with a higher thermal decomposition temperature is retained, thereby achieving the purpose of regulating the degree of pore opening of the molding agent. After the adsorbent is formed, the adsorption of ethane is greatly reduced while the amount of ethylene adsorption is basically maintained, thereby improving the thermodynamic selectivity of the material.
[0023] In summary, the molding method is simple in process, easy to control, highly compatible with existing industrial production lines, and the product obtained by this method has high mechanical strength and has prospects for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The X-ray diffraction patterns of the molding agents prepared in Example 1 of the present invention and the comparative example.
[0025] Figure 2 This is the single component adsorption isotherm of ethylene and ethane in Example 1 of the present invention.
[0026] Figure 3 It is the single component adsorption isotherm of ethylene and ethane in Comparative Example 1 of the present invention.
[0027] Depend on Figure 1 From the XRD diagram, it can be seen that the adsorbents after molding in Example 1 and Comparative Example 1 are similar to the standard spectra. Figure 1 Compared with Comparative Example 1, Example 1 is more consistent with the XRD pattern of the raw material, indicating that the physical phase of the activated molding agent is consistent with that of the raw material. Figure 2 It can be seen that the ethylene adsorption in Example 1 reaches 1.7 mmol / g, and the ethane adsorption reaches 0.34 mmol / g. Figure 3 It can be seen that the ethylene adsorption of Comparative Example 1 is 0.7 mmol / g, and the ethane adsorption is 0.45 mmol / g. DETAILED DESCRIPTION
[0028] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0029] The method for forming the ultra-microporous zinc-based MOF material provided by the present invention comprises the following steps:
[0030] (1) two or more binders with different thermal decomposition temperatures are stirred and mixed to form a composite binder; (2) the dried MOF material is mixed with the composite binder; (3) deionized water is added to the mixture of step (2) and mixed and stirred to obtain a paste, which is extruded to obtain a molding agent; (4) the molding agent is heated and activated in air, an inert atmosphere or a vacuum condition to remove part of the binder in the molding agent to obtain an activated molding agent.
[0031] In some embodiments, preferably, the mass ratio of the composite binder to the MOF material is (0.05-0.2):1.
[0032] In some embodiments, preferably, the thermal decomposition temperatures of various binders in the composite binder differ by more than 50°C.
[0033] In some embodiments, preferably, the composite binder includes a first binder and a second binder, and the thermal decomposition degree of the first binder is at least 50°C higher than that of the second binder; further preferably, the first binder is selected from at least one of pseudo-boehmite, silica sol, polyvinyl pyrrolidone, methyl cellulose, and polymethyl methacrylate; and the second binder is selected from at least one of polyvinyl alcohol, carboxymethyl cellulose, soluble starch, sucrose, glucose, and sodium alginate.
[0034] In some embodiments, preferably, the mass ratio of the first binder to the second binder is (0-1):1, and does not include 0.
[0035] In some embodiments, preferably, in step (3), the amount of deionized water added is 20 to 40 wt % of the mass of the mixture, and more preferably 20 to 25 wt %.
[0036] In some embodiments, preferably, the extrusion pressure of the extrusion molding is 70 to 250 kgf, and more preferably 90 to 120 kgf.
[0037] In some embodiments, preferably, the ultra-microporous zinc-based MOF material is cylindrical with a diameter of 2 to 4 mm and a length of 2 to 5 mm.
[0038] In some embodiments, preferably, the activation condition is: calcination at 200-350°C in an inert nitrogen atmosphere, and more preferably the temperature is 220-300°C.
[0039] In some embodiments, preferably, the thermal decomposition temperature of the ultra-microporous zinc-based MOF material is 300-500°C, and more preferably 370°C-420°C.
[0040] The ultra-microporous zinc-based MOF material of the present invention can be commercially available or synthesized according to existing methods.
[0041] Example 1
[0042] (1) Methyl cellulose and carboxymethyl cellulose are fully mixed in a ratio of 0.5:1 (mass ratio) to obtain a composite binder 1;
[0043] (2) 100 g of zinc-based ultra-microporous MOF powder and 10 g of composite binder 1 were mixed evenly, and the mixture was sieved through a 200-mesh sieve to obtain a mixture A;
[0044] (3) Add 25 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0045] (4) The obtained mixture B was extruded by an extruder, shaped into granules, and activated in a nitrogen atmosphere at 250° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0046] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.7 mmol / g, the ethane adsorption capacity was 0.34 mmol / g, and the ethylene selectivity of the material was 5.0.
[0047] Strength test of columnar particles: 20 tests and average value: 114.3N / cm
[0048] Example 2
[0049] (1) polyvinyl pyrrolidone and polyvinyl alcohol are fully mixed in a ratio of 0.3:1 (mass ratio) to obtain a composite binder 2;
[0050] (2) 100 g of zinc-based ultra-microporous MOF powder and 20 g of composite binder 2 were mixed evenly, and the mixture was sieved through a 200-mesh sieve to obtain a mixture A;
[0051] (3) adding 40 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0052] (4) The obtained mixture B is extruded by an extruder, shaped into granules, and activated in air at 300° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0053] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.66 mmol / g, the ethane adsorption capacity was 0.3 mmol / g, and the ethylene selectivity of the material was 5.5.
[0054] Strength test of columnar particles: 20 tests and average value: 102.5.N / cm
[0055] Example 3
[0056] (1) silica sol and soluble starch are fully mixed in a ratio of 0.25:1 (mass ratio) to obtain a composite binder 3;
[0057] (2) 100 g of zinc-based ultra-microporous MOF powder and 15 g of composite binder 3 were mixed evenly, and the mixture was sieved through a 200-mesh sieve to obtain a mixture A;
[0058] (3) Add 23 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0059] (4) The obtained mixture B was extruded by an extruder, shaped into granules, and vacuum activated at 350° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0060] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.74 mmol / g, the ethane adsorption capacity was 0.33 mmol / g, and the ethylene selectivity of the material was 5.3.
[0061] Strength test of columnar particles: 20 tests and average value: 132.5N / cm
[0062] Example 4
[0063] (1) Pseudo-boehmite and glucose are fully mixed in a ratio of 0.4:1 (mass ratio) to obtain a composite binder 4;
[0064] (2) 100 g of zinc-based ultra-microporous MOF powder and 20 g of composite binder 4 were mixed evenly, and then sieved through a 200-mesh sieve to obtain a mixture A;
[0065] (3) adding 40 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0066] (4) The obtained mixture B was extruded by an extruder, shaped into granules, and activated with nitrogen at 220° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0067] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.83 mmol / g, the ethane adsorption capacity was 0.41 mmol / g, and the ethylene selectivity of the material was 4.5.
[0068] Strength test of columnar particles: 20 tests and average value: 106.3N / cm
[0069] Example 5
[0070] (1) polymethyl methacrylate and sodium alginate are fully mixed in a ratio of 0.1:1 (mass ratio) to obtain a composite adhesive 5;
[0071] (2) 100 g of zinc-based ultra-microporous MOF powder and 5 g of composite binder 2 were mixed evenly, and the mixture was sieved through a 200-mesh sieve to obtain a mixture A;
[0072] (3) Add 21 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0073] (4) The obtained mixture B was extruded by an extruder, shaped into granules, and activated with nitrogen at 240° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0074] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.7 mmol / g, the ethane adsorption capacity was 0.4 mmol / g, and the ethylene selectivity of the material was 4.25.
[0075] Strength test of columnar particles: 20 tests and average value: 114.9N / cm
[0076] Example 6
[0077] (1) polyvinyl pyrrolidone and carboxymethyl cellulose are fully mixed in a ratio of 1:1 (mass ratio) to obtain a composite binder 6;
[0078] (2) 100 g of zinc-based ultra-microporous MOF powder and 10 g of composite binder 2 were mixed evenly, and the mixture was sieved through a 200-mesh sieve to obtain a mixture A;
[0079] (3) Add 27.5 g of deionized water dropwise to the mixture A obtained in step ②, stirring thoroughly to mix the mixture evenly, to obtain a mixture B;
[0080] (4) The obtained mixture B was extruded by an extruder, shaped into granules, and activated with nitrogen at 280° C. for 4 h to obtain columnar granules with a diameter of 2 mm.
[0081] The adsorption capacity of the columnar particles was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 1.88 mmol / g, the ethane adsorption capacity was 0.46 mmol / g, and the ethylene selectivity of the material was 4.1.
[0082] Strength test of columnar particles: 20 tests and average value: 101.6N / cm
[0083] Comparative Example 1
[0084] The preparation method and composition of the molded body are the same as those of Example 1, except that the obtained zinc-based ultra-microporous MOF material is not activated.
[0085] The adsorption capacity was tested using an intelligent weight adsorption instrument. The ethylene adsorption capacity was 0.7 mmol / g, the ethane adsorption capacity was 0.45 mmol / g, and the ethylene selectivity of the material was 1.5.
[0086] Test the strength of the molding agent: Test 20 times and take the average value: 130.7N / cm
[0087] Comparative Example 2
[0088] The preparation method of the forming agent is the same as that of Example 1, except that methyl fiber is used instead of the mixed binder to obtain a forming agent for the zinc-based ultra-microporous MOF material, wherein the forming agent is a columnar particle with a diameter of 2 mm.
[0089] The molding agent strength test was carried out: the average value of 20 tests was 36.7 N / cm, and the strength was significantly lower than that of Example 1.
[0090] Comparative Example 3
[0091] The preparation method and composition of the molded body are the same as those of Example 1, except that the molding agent of the obtained zinc-based ultra-microporous MOF material is calcined and activated at 370°C.
[0092] The activated molding agent will break into pieces with a slight pinch, so it has no significance for strength testing.
[0093] The adsorption capacity was tested by an intelligent gravimetric adsorption instrument, and the ethylene adsorption capacity was 1.5mmol / g, the ethane adsorption capacity was 1.13mmol / g, and the ethylene selectivity of the material was 1.3. The ethylene and ethane adsorption capacity was slightly reduced. In addition to the test error factor, the possible reason is that the crystal structure of the material was partially changed under high temperature roasting.
[0094] It can be seen from the above embodiments and comparative examples that the molding method of the ultra-microporous zinc-based MOF material provided by the present invention has the following advantages:
[0095] (1) The activated molding agent obtained not only has high mechanical strength, but also solves the problem of reduced material adsorption and poor selectivity caused by pore blockage by the binder.
[0096] (2) Since the composite binder is composed of two or more binders with different thermal decomposition temperatures, the binder with a lower thermal decomposition temperature can be removed in a controllable manner by controlling the calcination temperature, while the binder with a higher thermal decomposition temperature is retained, thereby achieving the purpose of regulating the degree of pore opening of the molding agent. After the adsorbent is formed, the adsorption of ethane is greatly reduced while the amount of ethylene adsorption is basically maintained, thereby improving the thermodynamic selectivity of the material.
[0097] In summary, the molding method is simple in process, easy to control, highly compatible with existing industrial production lines, and the product obtained by this method has high mechanical strength and has prospects for large-scale industrial application.
[0098] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A method for forming an ultra-microporous zinc-based MOF material, characterized in that: The following steps are involved: (1) stirring and mixing two or more binders with different thermal decomposition temperatures to form a composite binder; (2) mixing the dried MOF material and the composite binder to form a composite binder; (3) adding deionized water to the mixture of step (2) and stirring to obtain a paste, extruding and molding the paste to obtain a molding agent; (4) heating and activating the molding agent in air, an inert atmosphere or a vacuum condition to remove part of the binder in the molding agent to obtain an activated molding agent; The composite binder includes a first binder and a second binder, wherein the first binder is selected from at least one of pseudo-boehmite, silica sol, polyvinyl pyrrolidone, and polymethyl methacrylate; and the second binder is selected from at least one of carboxymethyl cellulose, soluble starch, sucrose, glucose, and sodium alginate.
2. The molding method according to claim 1, characterized in that: The mass ratio of the composite binder to the MOF material is (0.05-0.2):
1.
3. The molding method according to claim 1, characterized in that: The thermal decomposition temperatures of various binders in the composite binder differ by more than 50°C.
4. The molding method according to claim 1, characterized in that: The mass ratio of the first binder to the second binder is (0-1):1, and does not include 0.
5. The molding method according to claim 1, characterized in that: In step (3), the amount of deionized water added is 20 to 40 wt % of the mass of the mixture.
6. The molding method according to claim 5, characterized in that: In step (3), the amount of deionized water added is 20 to 25 wt % of the mass of the mixture.
7. The molding method according to claim 1, characterized in that: The extrusion pressure of the extrusion molding is 70 to 250 kgf.
8. The molding method according to claim 7, characterized in that: The extrusion pressure of the extrusion molding is 90-120 kgf.
9. The molding method according to claim 1, characterized in that: The ultra-microporous zinc-based MOF material is cylindrical, with a diameter of 2 to 4 mm and a length of 2 to 5 mm.
10. The molding method according to claim 1, characterized in that: The activation conditions are: calcination at 200-350° C. in an inert nitrogen atmosphere.
11. The molding method according to claim 10, characterized in that: The activation conditions are: calcination at 220-300° C. in an inert nitrogen atmosphere.
12. The molding method according to claim 1, characterized in that: The thermal decomposition temperature of the ultra-microporous zinc-based MOF material is 300-500°C.
13. The molding method according to claim 12, characterized in that: The thermal decomposition temperature of the ultra-microporous zinc-based MOF material is 370°C-420°C.