A heterojunction photocatalytic material with hierarchical structure and preparation method thereof

By constructing CuBi2O4/Bi2O2CO3 heterojunction materials, the problem of low utilization of visible light by photocatalytic materials is solved, efficient removal of the antibiotic tetracycline hydrochloride and energy consumption reduction are achieved, and a low-cost and efficient water pollution treatment solution is provided.

CN116408117BInactive Publication Date: 2024-10-18CHENGDU UNIVERSITY OF TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310228436.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photocatalytic materials have a low utilization rate of visible light and a high recombination rate of photogenerated carriers, resulting in low removal efficiency of the antibiotic tetracycline hydrochloride in water and high energy consumption during the preparation process.

Method used

By constructing a hierarchical structure heterojunction of three-dimensional CuBi2O4 and two-dimensional Bi2O2CO3, a CuBi2O4/Bi2O2CO3 composite material is formed, which broadens the photoresponse range, improves the photocatalytic oxidation ability, and adopts a simple and controllable preparation method, using low-power LED lamps for photocatalysis degradation.

Benefits of technology

It significantly improves the removal efficiency of the antibiotic tetracycline hydrochloride, reduces the energy consumption of the photocatalytic process, and achieves efficient adsorption-photocatalytic synergistic removal under natural light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116408117B_ABST
    Figure CN116408117B_ABST
Patent Text Reader

Abstract

The present invention relates to a CuBi 2 O 4 / Bi 2 O 2 CO 3 The invention relates to a heterojunction composite photocatalytic material and a preparation method thereof, belonging to the technical field of water pollution treatment and functional materials. 2 O 4 / Bi 2 O 2 CO 3 The composite material is prepared by low temperature chemical method in CuBi 2 O 4 In situ growth of Bi on microspheres 2 O 2 CO 3 The nanosheets were prepared, and then a Z-type heterojunction was constructed to form a 3D / 2D hierarchical structure. The composite material can adsorb organic pollutants in water and effectively degrade them using visible light. After 90 minutes of visible light irradiation, CuBi 2 O 4 / Bi 2 O 2 CO 3 The degradation rate of tetracycline hydrochloride solution with a concentration of 20 mg / L reached 90%. The process of the present invention is simple and controllable, and has low requirements on equipment. 2 O 4 / Bi 2 O 2 CO 3 Adsorption-visible light catalytic materials are of great significance to environmental governance and green energy utilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a heterojunction composite photocatalytic material with a hierarchical structure and a preparation method thereof, and belongs to the technical field of water pollutant treatment and functional materials. Background Art

[0002] With the rapid development of urbanization and industrialization, the ecological environment, especially the water environment, has been harmed by harmful organic compounds. Due to the widespread use of antibiotics in animal husbandry, aquaculture and clinical medicine, it is easy for their originals and metabolites to enter the water environment, making them a new organic pollutant. Among them, tetracycline hydrochloride (TCH) has become one of the most widely used antibiotics due to its high antibacterial activity, low price and few side effects. TCH has stable chemical properties and is difficult to be metabolized by human or animal bodies. Unmetabolized TCH will flow into natural environments such as water bodies, posing a potential threat to the ecological environment and human health. Therefore, many technologies for removing TCH from water bodies have been developed one after another, such as adsorption, biodegradation, electrochemical, photocatalytic oxidation, etc. The adsorption method has the risk of secondary pollution, the biodegradation method is easy to destroy the balance of the ecosystem, and the electrochemical method has high operating costs. Photocatalytic technology, as a green oxidation technology without secondary pollution, can degrade antibiotic macromolecules into water and carbon dioxide based on the use of solar energy by photocatalytic materials, thereby achieving complete removal of antibiotics, and has shown great potential in treating water pollution. However, photocatalytic technology also has certain limitations, such as difficulty in enriching pollutants, low utilization of visible light, and high recombination rate of photogenerated carriers. In order to circumvent the shortcomings of a single treatment technology, the rational combination of adsorption and photocatalytic technology is regarded as a potential strategy for more effective removal of TCH. The advantage of this strategy is that it can enrich TCH molecules on the catalyst surface through adsorption, thereby achieving efficient photocatalytic oxidation reactions, and photocatalytic technology can eliminate the risk of secondary pollution caused by adsorption, thereby reducing energy consumption. Therefore, by utilizing the synergistic effect between adsorption and photocatalytic technology, the development of photocatalysts with excellent adsorption-photocatalytic activity is expected to achieve more efficient removal of TCH in water bodies.

[0003] As a member of the bismuth (III) semiconductor family, Bi2O2CO3 exhibits a wide band gap (about 3.3 eV) that makes it only responsive to ultraviolet light. The low utilization rate of solar energy and the easy recombination of photogenerated carriers limit its practical photocatalytic application. In response to the above problems, it has been proven to be a simple and effective method to construct a heterojunction by coupling with other semiconductors, especially narrow-bandgap semiconductors. The composite material can exhibit excellent photocatalytic activity under visible light by combining two semiconductors to construct a heterojunction. In addition, by precisely controlling the structure of the composite material of different sizes, the composite material can also provide a larger specific surface area and more active sites, thereby enhancing the adsorption-photocatalytic synergistic removal of TCH from water by the photocatalyst. Among narrow-bandgap semiconductors, CuBi2O4 is regarded as a highly promising candidate material due to its strong response to visible light, matching band structure and controllable morphology.

[0004] Some materials that combine photocatalytic semiconductors with Bi2O2CO3 for TCH removal have been reported in the prior art. For example, Chinese patent document with publication number CN112138693A reports that flower-shaped Bi2O2CO3 is first prepared, and then Bi2O2CO3 is mixed with HAuCl4·4H2O and calcined to obtain Au / Bi2O2CO3 / Bi2O3 composite material. The composite material prepared by this method uses precious metal Au to modify the semiconductor, which increases the production cost and is not only used for degrading organic dyes; Chinese patent document with publication number CN109261193A reports that flower-shaped Bi2O2CO3 is first prepared, and then Bi2O2CO3 is mixed with HAuCl4·4H2O and calcined to obtain Au / Bi2O2CO3 / Bi2O3 composite material. The precursor solution of g-C3N4 and Bi2O2CO3 is mixed, and then subjected to ultrasound and solvent thermal treatment to obtain a composite material. The composite material prepared by this method uses a 300W xenon lamp for photocatalytic degradation, and the operating equipment has high power and energy consumption. The Chinese patent document with publication number CN113694946A reports a core-shell structure Bi2O2CO3 / rGO composite material for removing antibiotics from water. The formation of the core-shell structure enhances the adsorption of antibiotics, but a 200W to 500W mercury lamp is required for long-term ultraviolet light treatment during the preparation process, which increases energy consumption.

[0005] Therefore, it is particularly important to prepare a material that can effectively absorb visible light, has good adsorption photocatalytic effect, and consumes low energy during degradation for use in wastewater treatment.

[0006] The present invention successfully constructs a heterojunction with a hierarchical structure for the first time by combining three-dimensional (3D) CuBi2O4 with two-dimensional (2D) Bi2O2CO3. The CuBi2O4 / Bi2O2CO3 heterojunction composite material exhibits enhanced removal performance, which is attributed to the 3D / 2D hierarchical structure providing more active sites for the adsorption and photocatalytic degradation of pollutants. The formed heterojunction improves the utilization of visible light and promotes the rapid separation of photogenerated carriers. Summary of the invention

[0007] The first technical problem solved by the present invention is to provide a heterojunction photocatalytic material that can both adsorb and have photocatalytic performance under natural light to synergistically remove TCH.

[0008] The CuBi2O4 / Bi2O2CO3 heterojunction composite material of the present invention has a 3D / 2D hierarchical structure, can provide abundant adsorption sites, CuBi2O4 and Bi2O2CO3 form a Z-type heterojunction, broadens the light response range, increases the photocatalytic oxidation ability under visible light, and greatly improves the efficiency of removing TCH.

[0009] The second technical problem solved by the present invention is to provide a method for preparing a heterojunction composite photocatalytic material with a hierarchical structure, comprising the following steps:

[0010] a. Dissolve bismuth nitrate (Bi(NO3)3·5H2O) and copper sulfate (CuSO4·5H2O) in dilute nitric acid (HNO3) solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly add sodium hydroxide (NaOH) solution dropwise into the beaker containing the mixed metal salt solution, adjust the pH value in the beaker, and continue stirring to form a green solution.

[0011] b. The green solution obtained in step a is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate and placed in an oven for hydrothermal reaction. After the hydrothermal process is completed, it is cooled to room temperature, and the obtained product is centrifuged, washed, and dried to obtain CuBi2O4.

[0012] c. Then, bismuth nitrate (Bi(NO3)3·5H2O) is dissolved in ethylene glycol to obtain a metal salt solution, sodium carbonate (Na2CO3) is dissolved in water to obtain an alkaline solution, and the alkaline solution is slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, and the mixture is continuously stirred in a constant temperature water bath. Finally, the mixture is centrifuged, washed, and dried to obtain a CuBi2O4 / Bi2O2CO3 composite material.

[0013] In one embodiment, in step a, the pH value of the solution is 12-14; preferably, the pH value of the solution is 13.

[0014] In one embodiment, in step b, the hydrothermal temperature is 160-200° C., and the hydrothermal time is 2-8 hours; preferably, the hydrothermal temperature is 180° C., and the hydrothermal time is 4 hours.

[0015] In one embodiment, in step c, the molar ratio of Bi(NO3)3·5H2O to Na2CO3 is 1:4 to 1:16; preferably, the molar ratio of Bi(NO3)3·5H2O to Na2CO3 is 1:8.

[0016] In one embodiment, in step c, the mass fraction of CuBi2O4 in the weight of CuBi2O4 / Bi2O2CO3 is 5% to 20%; preferably, the mass fraction of CuBi2O4 in the weight of CuBi2O4 / Bi2O2CO3 is 10%.

[0017] In one embodiment, in step c, the temperature of the constant temperature water bath is 30-50°C; preferably, the temperature of the constant temperature water bath is 40°C.

[0018] In one embodiment, in step c, the stirring time is 0.5 to 2 hours; preferably, the stirring time is 1 hour.

[0019] The third technical problem solved by the present invention is to provide an application of the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material with a hierarchical structure, which is used for removing TCH in water.

[0020] Beneficial effects of the present invention:

[0021] 1. The CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material of the present invention forms a 3D / 2D hierarchical structure by in-situ growth on CuBi2O4, providing more adsorption sites and broadening the light response range of the composite material. At the same time, with the help of the Z-type heterojunction formed by CuBi2O4 and Bi2O2CO3, the transfer and separation of photogenerated electrons and holes are promoted, so that the composite material has an excellent effect of adsorption-photocatalytic synergistic degradation of TCH under visible light, further improving the removal ability of TCH.

[0022] 2. The preparation method of the present invention has a simple and controllable process, and the raw materials used are from a wide range of sources. Low-power LED lamps are used for photocatalytic degradation of TCH, which has low energy consumption and is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD pattern of the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 1.

[0024] Figure 2 This is a diagram showing the removal efficiency of TCH by the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 1.

[0025] Figure 3 This is the UV-Vis spectrum of the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 2.

[0026] Figure 4This is a diagram showing the removal efficiency of TCH by the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 2.

[0027] Figure 5 This is the SEM image of the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 2.

[0028] Figure 6 This is the XRD pattern of the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 3.

[0029] Figure 7 This is a diagram showing the removal efficiency of TCH by the CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 3. DETAILED DESCRIPTION

[0030] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0031] Photocatalytic activity test

[0032] The degradation object is a TCH solution with a concentration of 20 mg / L. CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material is added to the reactor and stirred for 45 minutes under dark conditions to allow the reaction system in the solution to reach adsorption-desorption equilibrium. Subsequently, a 40W LED lamp is turned on for photocatalytic degradation. During the entire experimental process, samples are taken every 15 to 30 minutes, with 6 ml of sample taken each time. The samples are centrifuged to obtain the supernatant, and the TCH concentration is determined by UV-visible spectrophotometry. The absorbance value at a wavelength of 357nm is determined, and the removal rate of TCH is calculated.

[0033] Example 1

[0034] Synthesis process:

[0035] 1) Weigh 1.9403 g Bi(NO3)3·5H2O and 0.4994 g CuSO4·5H2O and dissolve them in 0.1 mol / L dilute HNO3 solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly add 2 mol / L NaOH solution dropwise into the beaker containing the mixed metal salt solution. Control the pH value in the beaker to 12 and continue stirring for 40 min to form a green solution.

[0036] 2) The green solution obtained in step 1) is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate, and then placed in an oven and heated at 160° C. for 8 h. After the hydrothermal treatment, it is cooled to room temperature, and the obtained product is centrifugally washed three times with deionized water and anhydrous ethanol, respectively, and dried in an oven to obtain CuBi2O4.

[0037] 3) According to the molar ratio of Bi(NO3)3·5H2O to Na2CO3 of 1:4, 1.9403g Bi(NO3)3·5H2O) was weighed and dissolved in 20ml ethylene glycol to obtain a metal salt solution, 1.6958g Na2CO3 was dissolved in water to obtain an alkaline solution, and the alkaline solution was slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, the mass fraction of CuBi2O4 in the weight of CuBi2O4 / Bi2O2CO3 was 20%, and the mixture was stirred continuously in a constant temperature water bath at 30°C for 2h, and finally centrifuged, washed and dried to obtain a CuBi2O4 / Bi2O2CO3 heterojunction composite material.

[0038] Figure 1 The XRD pattern of the 20%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material obtained in Example 1 of the present invention is shown in FIG. Figure 1 It can be seen that the XRD results of CuBi2O4 prepared in Example 1 are consistent with the standard diffraction peaks, the crystallinity is good and no other impurity peaks appear. The XRD spectrum of the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material shows the diffraction peaks of CuBi2O4 and Bi2O2CO3, indicating that the composite structure was successfully constructed under this growth condition.

[0039] Figure 2 This is a graph showing the removal efficiency of the 20%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material for TCH solution obtained in Example 1 of the present invention. Figure 2 It can be seen that the 20%-CuBi2O4 / Bi2O2CO3 composite material obtained in Example 1 has a removal rate of 82.44% for a 20 mg / L TCH solution within 135 min, and can effectively remove organic pollutants in the water environment.

[0040] Example 2

[0041] Synthesis process:

[0042] 1) Weigh 1.9403 g Bi(NO3)3·5H2O and 0.4994 g CuSO4·5H2O and dissolve them in 0.1 mol / L dilute HNO3 solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly add 2 mol / L NaOH solution dropwise into the beaker containing the mixed metal salt solution. The pH value in the beaker is controlled to be 13, and stirring is continued for 40 min to form a green solution.

[0043] 2) The green solution obtained in step 1) is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate, and then placed in an oven and heated at 180° C. for 4 h. After the hydrothermal treatment, it is cooled to room temperature, and the obtained product is centrifugally washed three times with deionized water and anhydrous ethanol, respectively, and dried in an oven to obtain CuBi2O4.

[0044] 3) According to the molar ratio of Bi(NO3)3·5H2O to Na2CO3 of 1:8, 1.9403g Bi(NO3)3·5H2O) was weighed and dissolved in 20ml ethylene glycol to obtain a metal salt solution, 3.3917g Na2CO3 was dissolved in water to obtain an alkaline solution, and the alkaline solution was slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, the mass fraction of CuBi2O4 in the weight of CuBi2O4 / Bi2O2CO3 was 10%, and the mixture was stirred continuously in a constant temperature water bath at 40°C for 1h. Finally, the mixture was centrifuged, washed and dried to obtain a CuBi2O4 / Bi2O2CO3 heterojunction composite material.

[0045] Figure 3 The UV-Vis spectrum of the 10%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material prepared in Example 2 of the present invention is shown in FIG. Figure 3 It can be seen that the absorption wavelength of the 10%-CuBi2O4 / Bi2O2CO3 heterojunction composite material prepared in Example 2 is red-shifted compared with that of Bi2O2CO3 alone, and the light response range is broadened to the visible light region.

[0046] Figure 4 This is a graph showing the removal efficiency of the 10%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material for TCH solution obtained in Example 2 of the present invention. Figure 4 It can be seen that the 10%-CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 2 has a removal rate of 90.01% for a TCH solution with a concentration of 20 mg / L within 135 minutes, achieving basic removal of organic pollutants in the water environment.

[0047] Figure 5 This is a SEM image of the 10%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material obtained in Example 2 of the present invention. Figure 5 It can be seen that the prepared heterojunction catalyst presents a spherical structure, and irregularly shaped nanosheets can be observed on the surface of CuBi2O4 microspheres, which are Bi2O2CO3 nanosheets. Figure 5 It was further demonstrated that Bi2O2CO3 flakes wrapped CuBi2O4 microspheres over a large area, indicating the successful synthesis of CuBi2O4 / Bi2O2CO3 heterojunction photocatalyst with 3D / 2D hierarchical structure.

[0048] Example 3

[0049] Synthesis process:

[0050] 1) Weigh 1.9403 g Bi(NO3)3·5H2O and 0.4994 g CuSO4·5H2O and dissolve them in 0.1 mol / L dilute HNO3 solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly add 2 mol / L NaOH solution dropwise into the beaker containing the mixed metal salt solution. Control the pH value in the beaker to 14 and continue stirring for 40 min to form a green solution.

[0051] 2) The green solution obtained in step 1) is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate, and then placed in an oven and heated at 200° C. for 2 h. After the hydrothermal process is completed, it is cooled to room temperature, and the obtained product is centrifugally washed three times with deionized water and anhydrous ethanol, respectively, and dried in an oven to obtain CuBi2O4.

[0052] 3) According to the molar ratio of Bi(NO3)3·5H2O to Na2CO3 of 1:16, 1.9403g Bi(NO3)3·5H2O) was weighed and dissolved in 20ml ethylene glycol to obtain a metal salt solution, 6.7834g Na2CO3 was dissolved in water to obtain an alkaline solution, and the alkaline solution was slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, the mass fraction of CuBi2O4 in the weight of CuBi2O4 / Bi2O2CO3 was 5%, and the mixture was continuously stirred for 0.5h in a constant temperature water bath at 50°C, and finally centrifuged, washed and dried to obtain a CuBi2O4 / Bi2O2CO3 heterojunction composite material.

[0053] Figure 6 The XRD pattern of the 5%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material obtained in Example 3 of the present invention is shown in FIG. Figure 6 It can be seen that the XRD results of CuBi2O4 prepared in Example 3 are consistent with the standard diffraction peaks, the crystallinity is good and no other impurity peaks appear. The XRD spectrum of the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material shows the diffraction peaks of CuBi2O4 and Bi2O2CO3, indicating that the composite structure was successfully constructed under this growth condition.

[0054] Figure 7 This is a graph showing the removal efficiency of the 5%-CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material for TCH solution obtained in Example 3 of the present invention. Figure 7It can be seen that the 5%-CuBi2O4 / Bi2O2CO3 heterojunction composite material obtained in Example 3 has a removal rate of 86.24% for a TCH solution with a concentration of 20 mg / L within 135 minutes, and can effectively remove organic pollutants in the water environment.

Claims

1. A CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material with a hierarchical structure, characterized in that: The preparation method of the photocatalytic material comprises the following steps: a. Dissolve Bi(NO3)3·5H2O and CuSO4·5H2O in dilute nitric acid (HNO3) solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly drop sodium hydroxide (NaOH) solution into the beaker containing the mixed metal salt solution, adjust the pH value in the beaker, and continue stirring to form a green solution. b. The green solution obtained in step a is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate, and placed in an oven for hydrothermal reaction. After the hydrothermal reaction is completed, the solution is cooled to room temperature, and the obtained product is centrifuged, washed, and dried to obtain CuBi2O4; c. Then, Bi(NO3)3·5H2O is dissolved in ethylene glycol to obtain a metal salt solution, sodium carbonate (Na2CO3) is dissolved in water to obtain an alkaline solution, and the alkaline solution is slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, and the mixture is continuously stirred in a constant temperature water bath, and finally centrifuged, washed, and dried to obtain a CuBi2O4 / Bi2O2CO3 composite material, wherein the mass fraction of CuBi2O4 to the weight of CuBi2O4 / Bi2O2CO3 is 5% to 20%.

2. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 1, characterized in that: The following steps are involved: a. Dissolve Bi(NO3)3·5H2O and CuSO4·5H2O in dilute nitric acid (HNO3) solution to obtain a mixed metal salt solution. Then, under continuous stirring, slowly drop sodium hydroxide (NaOH) solution into the beaker containing the mixed metal salt solution, adjust the pH value in the beaker, and continue stirring to form a green solution. b. The green solution obtained in step a is transferred to a stainless steel autoclave with a polytetrafluoroethylene substrate, and placed in an oven for hydrothermal reaction. After the hydrothermal reaction is completed, the solution is cooled to room temperature, and the obtained product is centrifuged, washed, and dried to obtain CuBi2O4; c. Then, Bi(NO3)3·5H2O is dissolved in ethylene glycol to obtain a metal salt solution, sodium carbonate (Na2CO3) is dissolved in water to obtain an alkaline solution, and the alkaline solution is slowly added dropwise to a single-necked flask containing the metal salt solution and CuBi2O4, and the mixture is continuously stirred in a constant temperature water bath, and finally centrifuged, washed, and dried to obtain a CuBi2O4 / Bi2O2CO3 composite material, wherein the mass fraction of CuBi2O4 to the weight of CuBi2O4 / Bi2O2CO3 is 5% to 20%.

3. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step a, the solution pH value is 12-14.

4. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step b, the hydrothermal temperature is 160-200°C.

5. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step b, the hydrothermal time is 2 to 8 hours.

6. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step c, the molar ratio of Bi(NO3)3·5H2O to Na2CO3 is 1:4 to 1:

16.

7. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step c, the temperature of the constant temperature water bath is 30-50°C.

8. The method for preparing the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 2, characterized in that: In step c, the stirring time is 0.5 to 2 hours.

9. An application of the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material according to claim 1 or the CuBi2O4 / Bi2O2CO3 heterojunction composite photocatalytic material prepared by the preparation method according to any one of claims 2 to 8, characterized in that: It was used for efficient adsorption and degradation of tetracycline hydrochloride in water under visible light.

Citation Information

Patent Citations

  • Method for synthesizing Bi2O2CO3 / g-C3N4 flower-like compound photocatalyst on basis of ultrasound-solvent thermal approach and application of photocatalyst

    CN109261193A

  • Preparation method of flower-like Au / Bi2O2CO3 / Bi2O3 photocatalyst

    CN112138693A

  • Bi2O2CO3@rGO photocatalyst with core-shell structure as well as preparation method and application thereof

    CN113694946A

  • Copper bismuthate / bismuthyl carbonate heterojunction photocatalyst as well as preparation method and application thereof

    CN115069282A