A secondary growth preparation method for nano lithium iron phosphate
By adopting the secondary growth method of nano-lithium iron phosphate and two-dimensional phosphorus element in the preparation of lithium iron phosphate, the problems of complex preparation and poor controllability of lithium iron phosphate in the existing technology are solved, and high-rate performance and pure phase materials are achieved. The preparation is suitable for industrial production.
Patent Information
- Application Number
- CN202310407851.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-17
AI Technical Summary
The existing preparation method of lithium iron phosphate is complex and lacks controllability, resulting in unclear advantageous channels for lithium ion transmission, and may introduce impurities, affecting its rate performance and safety.
Nano-lithium iron phosphate is used as a seed crystal, and two-dimensional phosphorus is introduced for secondary growth through a hydrothermal reaction. The crystal face exposure rate is controlled to achieve the preparation of pure-phase lithium iron phosphate cathode materials with high rate performance.
The lithium iron phosphate material obtained by the secondary growth method has an improved lithium ion channel structure, improves rate performance, simplifies the process, reduces energy consumption, and avoids the introduction of impurities, making it suitable for industrial production.
Smart Images

Figure CN116409772B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, and in particular to a secondary growth preparation method for nano lithium iron phosphate. Background Art
[0002] Lithium iron phosphate is a positive electrode material for lithium-ion batteries. It has high safety, stability, cycle life and energy density, so it has been widely used in portable electronic devices, electric vehicles, energy storage systems and other fields. Compared with traditional lithium cobalt oxide, lithium nickel oxide and ternary materials, it has higher safety and environmental protection, and is more suitable for large-scale applications. However, due to its low lithium ion migration rate and electronic conductivity, its rate performance is poor. At present, nano-sizing, doping and coating of lithium iron phosphate are important methods to improve its rate performance.
[0003] Chinese patent CN115367724A discloses a method for producing lithium iron phosphate material using biomass agent, firstly, the lithium source, iron source and phosphorus source are ground into an aqueous solution, and a mixture of biomass agent and benzenesulfonic acid is added as an additive, then the materials prepared in the first two steps are mixed according to the proportion for hydrothermal reaction, and finally the material is eluted to obtain lithium iron phosphate powder. Similarly, Chinese patent CN102013490A discloses a high-rate performance lithium iron phosphate positive electrode material and its preparation method, the ball-milled graphite is mixed with iron salt, phosphate and lithium salt, and anhydrous ethanol is used as a medium for secondary ball milling, the powder material obtained by slurry spray drying is then placed in a rotary furnace for atmosphere sintering to obtain a high-rate performance lithium iron phosphate positive electrode material. In addition, Chinese patent CN114171740A discloses a method for preparing a nano lithium iron phosphate positive electrode material, firstly, hollow nano carbon balls are prepared, then mixed with lithium salt, iron salt and phosphorus salt to form a reaction solution, and hydrothermally reacted under inert gas to obtain a lithium iron phosphate precursor, and finally roasted. The above method is relatively cumbersome and lacks controllability over the lithium iron phosphate nanostructure, especially the lithium ion transmission advantage channel. In addition, it may introduce some impurities that cannot be removed, which brings uncontrollable potential risks to its application. Therefore, it is urgent to develop a new lithium iron phosphate preparation method to achieve the regulation of lithium iron phosphate structure and performance. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a secondary growth preparation method of nano lithium iron phosphate, which uses primary nano lithium iron phosphate as a seed, introduces a two-dimensional phosphorus element and a lithium iron phosphate precursor, and utilizes the two-dimensional phosphorus element to induce the seed to grow secondary in a hydrothermal process to achieve dominant crystal plane regulation. The present invention synthesizes a pure-phase lithium iron phosphate positive electrode material with high rate performance through a simple process, thereby solving the problem of impurities in the lithium iron phosphate preparation process in the prior art.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] In one aspect, the present invention provides a method for preparing secondary growth of nano lithium iron phosphate, comprising the following steps:
[0007] Nano lithium iron phosphate as a seed, two-dimensional phosphorus and a reducing agent are subjected to hydrothermal reaction in a lithium iron phosphate precursor solution; the lithium iron phosphate precursor solution comprises an iron source, a lithium source and a phosphorus source.
[0008] As a preferred embodiment, the reaction temperature of the hydrothermal reaction is 150° C. to 220° C.; the insulation time of the hydrothermal reaction is 150 min to 220 min.
[0009] As a preferred embodiment, the reducing agent is ascorbic acid.
[0010] As a preferred embodiment, the iron source is a water-soluble ferrous salt, preferably ferrous sulfate heptahydrate;
[0011] Preferably, the lithium source is a water-soluble lithium salt, preferably lithium hydroxide monohydrate;
[0012] Preferably, the phosphorus source is a water-soluble phosphorus source, preferably phosphoric acid;
[0013] Preferably, the solvent of the lithium iron phosphate precursor solution is a mixed solvent of water and ethylene glycol.
[0014] As a preferred embodiment, the two-dimensional phosphorus element is two-dimensional black phosphorus;
[0015] Preferably, the lateral size of the two-dimensional phosphorus single substance is 0.5 μm to 100 μm, and the thickness is 1 nm to 30 nm.
[0016] As a preferred embodiment, the mass ratio of the two-dimensional phosphorus element to the nano-lithium iron phosphate as a seed crystal is 1:0.4-5;
[0017] Preferably, in the lithium iron phosphate precursor solution, the molar ratio of iron in the iron source, lithium in the lithium source, and phosphorus in the phosphorus source is 1:3-4:1-2;
[0018] Preferably, the mass ratio of the reducing agent to the iron source is 1 to 2:2780;
[0019] Preferably, the mass ratio of the nano-lithium iron phosphate used as the seed crystal to the iron source is 1-10:125.
[0020] In some specific embodiments, the secondary growth preparation method further includes post-treatments of cooling, washing, and drying, wherein the cooling can be carried out in a natural cooling manner.
[0021] In the technical solution of the present invention, the mass ratio of the theoretical mass of the nano-lithium iron phosphate obtained by the above-mentioned secondary growth preparation method to the mass ratio of the nano-lithium iron phosphate used as the seed crystal is 5 to 200:1.
[0022] As a preferred embodiment, the nano lithium iron phosphate used as the seed crystal is prepared by a hydrothermal method;
[0023] Preferably, the particle size of the nano-lithium iron phosphate used as the seed crystal is 30 nm to 200 nm.
[0024] In certain specific embodiments, the hydrothermal method for preparing nano lithium iron phosphate as a seed crystal comprises the following steps:
[0025] A solution including a reducing agent, an iron source, a lithium source and a phosphorus source is subjected to a hydrothermal reaction. The reducing agent is ascorbic acid; the iron source is a water-soluble ferrous salt, preferably ferrous sulfate heptahydrate; the lithium source is a water-soluble lithium salt, preferably lithium hydroxide monohydrate; the phosphorus source is a water-soluble phosphorus source, preferably phosphoric acid; and the solvent of the lithium iron phosphate precursor solution is a mixed solvent of water and ethylene glycol. The conditions of the hydrothermal reaction are 150°C to 220°C for 150min to 220min.
[0026] In another aspect, the present invention provides nano lithium iron phosphate obtained by the above secondary growth preparation method.
[0027] In another aspect, the present invention provides the use of the nano lithium iron phosphate in preparing lithium ion batteries, specifically, the use of the nano lithium iron phosphate in preparing positive electrode materials for lithium ion batteries.
[0028] The above technical solution has the following advantages or beneficial effects: the present invention uses nano lithium iron phosphate as a seed crystal and adds a two-dimensional phosphorus element as a regulator through a hydrothermal method to obtain lithium iron phosphate with different crystal surface exposure rates through secondary in-situ growth, wherein the two-dimensional phosphorus element can construct a microenvironment through redox reactions to achieve secondary growth regulation of lithium iron phosphate.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] 1. Innovation in the regulation mechanism: The two-dimensional phosphorus element undergoes an oxidation reaction during the hydrothermal process, and the surface becomes negatively charged, attracting crystal seeds and positive ions. The local ion concentration on the black phosphorus surface increases, thereby regulating the growth of lithium iron phosphate on the crystal seeds, ultimately achieving the purpose of changing the crystal surface exposure rate;
[0031] 2. The more the crystal surface of the lithium ion channel is exposed, the shorter the channel distance is, the better the performance is. The seed crystal is affected by the two-dimensional phosphorus element and can achieve the effect of a larger proportion of the channel crystal surface (010) and a relatively shorter channel distance through secondary growth;
[0032] 3. The secondary grown lithium iron phosphate material is synthesized by a low-temperature hydrothermal method, which has low energy consumption, simple equipment and operation, no introduction of other organic compounds, easy elution, and is conducive to the industrial production of high-performance nano lithium iron phosphate. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a scanning electron microscope image of the nano lithium iron phosphate seed prepared in Manufacturing Example 1 of the present invention.
[0034] Figure 2 It is a scanning electron microscope image of the lithium iron phosphate prepared in Comparative Examples 1 and 3 of the present invention.
[0035] Figure 3 It is the X-ray diffraction pattern of the lithium iron phosphate prepared in Comparative Examples 1-2 and Example 1 of the present invention.
[0036] Figure 4 is a scanning electron microscope image of the lithium iron phosphate prepared in Example 1 of the present invention.
[0037] Figure 5 It is a rate performance diagram of the lithium iron phosphate prepared in Comparative Example 2 and Example 1 of the present invention.
[0038] Figure 6 It is a charge and discharge curve diagram of the lithium iron phosphate prepared in Example 1 of the present invention under 15C charge and discharge conditions. DETAILED DESCRIPTION
[0039] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0040] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0041] Production Example 1
[0042] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, add them to 12 mL of ethylene glycol, and finally add them to the autoclave;
[0043] Step 2, heating to 180°C and keeping warm for 60 minutes;
[0044] Step 3: After natural cooling, wash with pure water for several times and then dry to obtain nano lithium iron phosphate seed crystals.
[0045] The nano lithium iron phosphate seeds obtained in this manufacturing example are as follows Figure 1 As shown, the particle size of the seed crystal is 30nm to 200nm.
[0046] Comparative Example 1
[0047] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 10 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, add them to 12 mL of ethylene glycol, and finally add them to the autoclave;
[0048] Step 2, heating to 180°C and keeping warm for 200 minutes;
[0049] Step 3: After natural cooling, wash with pure water several times to obtain lithium iron phosphate.
[0050] like Figure 2 As shown, the pure phase lithium iron phosphate material can be obtained in this comparative example, and the particles of the seed crystals become significantly larger after the secondary growth. The X-ray diffraction pattern of the lithium iron phosphate material prepared in this comparative example is shown in FIG. Figure 3 As shown, the XRD test results of the samples correspond to the standard cards.
[0051] Comparative Example 2
[0052] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, mix them and add them to 12 mL of ethylene glycol, and finally add them to the autoclave;
[0053] Step 2, heating to 180°C and keeping warm for 200 minutes;
[0054] Step 3: After natural cooling, wash with pure water several times to obtain a pure phase lithium iron phosphate material.
[0055] The XRD test diagram of the pure phase lithium iron phosphate material obtained in this comparative example is shown in Figure 3 .
[0056] Comparative Example 3
[0057] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, mix them and add them to 12 mL of ethylene glycol containing 20 mg of black phosphorus, and finally add them to the autoclave;
[0058] Step 2, heating to 180°C and keeping warm for 200 minutes;
[0059] Step 3: After natural cooling, wash with pure water several times to obtain a pure phase lithium iron phosphate material.
[0060] like Figure 2 As shown, this comparative example shows that the particle size distribution of the synthesized lithium iron phosphate is extremely uneven.
[0061] Example 1
[0062] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 8 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, mix them and add them into 12 mL of ethylene glycol containing 20 mg of black phosphorus, and finally add them into a high-pressure reactor;
[0063] Step 2, heating to 180°C and keeping warm for 200 minutes;
[0064] Step three, after natural cooling, wash with pure water several times to obtain the secondary grown lithium iron phosphate.
[0065] The X-ray diffraction pattern of the pure phase lithium iron phosphate material prepared in this example is as follows Figure 3 As shown in Figure 2, the XRD test results of the samples correspond to those of the standard cards. Figure 3 It can be seen that in Example 1, the exposure ratio of the (020) crystal plane to the (200) crystal plane of the lithium iron phosphate material in XRD is larger than that in Comparative Examples 1 and 2, which means that the more (010) is exposed in the advantageous direction of lithium ion transmission, the more conducive it is to lithium ion migration, which helps to improve the rate performance.
[0066] Figure 4 Shown is a scanning electron microscope image of the lithium iron phosphate material prepared in this example.
[0067] The lithium iron phosphate material prepared in this embodiment and comparative example 2 is first carbonized, and the carbonization process is carried out according to the reference [Ind.Eng.Chem.Res.2017,56,10648-10657]. The specification of the button half-cell is CR2032, and the half-cell slurry is prepared as follows: the carbonized lithium iron phosphate is mixed with superconducting carbon black (SP) at a weight ratio of 8:1, and after sufficient grinding, a polyvinylidene fluoride N-methylpyrrolidone (PVDF / NMP) solution is added to the ground powder. At this time, the mass ratio of carbonized lithium iron phosphate: SP: PVDF is 8:1:1, and then coated on aluminum foil, and dried at 120°C for 6 hours under vacuum conditions, and then cut into 12mm diameter positive electrode sheets for use. Prepare the positive electrode shell, diaphragm, spring, gasket, lithium sheet, negative electrode shell and weighed positive electrode sheet. In this experiment, lithium sheet was used as negative electrode, Celgard 2400 microporous membrane was used as separator, 3 to 4 drops of lithium hexafluorophosphate electrolyte were dripped on both sides of the separator by pipette gun, and the battery was installed in a glove box filled with argon gas. After installation, the battery was packaged using an electric packaging machine. After the half-battery was made and left to stand for 12 hours, the rate performance was tested. The charge and discharge range was 2.0~3.75V, 1C=170mA / g. The rate performance diagram of the half-battery prepared by the same method in this embodiment and comparative example 2 is shown in the figure below: Figure 5 The charge and discharge curve of the half-cell prepared in this embodiment at 15C is shown in Figure 6 As shown in the figure, it can be seen that the half-cell prepared in this embodiment has good charge-discharge performance and rate performance, which is significantly better than that of comparative example 2.
[0068] Example 2
[0069] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the above ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 50 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 100 μL of phosphoric acid, mix them and add them into 12 mL of ethylene glycol containing 10 mg of black phosphorus, and finally add them into a high-pressure reactor;
[0070] Step 2, heating to 150°C and keeping warm for 180 minutes;
[0071] Step three, after natural cooling, wash with pure water several times to obtain the secondary grown lithium iron phosphate.
[0072] Example 3
[0073] Step 1, prepare 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.6 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.3 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 20 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 80 μL of phosphoric acid, mix them and add them into 12 mL of ethylene glycol containing 10 mg of black phosphorus, and finally add them into the autoclave;
[0074] Step 2, heating to 180°C and keeping warm for 220 minutes;
[0075] Step three, after natural cooling, wash with pure water several times to obtain the secondary grown lithium iron phosphate.
[0076] Example 4
[0077] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.3 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 15 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 100 μL of phosphoric acid, mix them and add them into 12 mL of ethylene glycol containing 5 mg of black phosphorus, and finally add them into a high-pressure reactor;
[0078] Step 2, heating to 150°C and keeping warm for 220 minutes;
[0079] Step three, after natural cooling, wash with pure water several times to obtain the secondary grown lithium iron phosphate.
[0080] Example 5
[0081] Step 1, prepare a 0.1 mg / mL ascorbic acid aqueous solution, weigh 2.78 g of ferrous sulfate heptahydrate and dissolve it in 10 mL of the ascorbic acid aqueous solution; weigh 1.4 g of lithium hydroxide monohydrate and prepare it into 10 mL of aqueous solution; take 70 mg of the seed crystals prepared in Manufacturing Example 1, 3 mL of the ferrous sulfate solution prepared above, 3 mL of lithium hydroxide solution and 100 μL of phosphoric acid, mix them and add them into 12 mL of ethylene glycol containing 30 mg of black phosphorus, and finally add them into a high-pressure reactor;
[0082] Step 2, heating to 220°C and keeping warm for 220 minutes;
[0083] Step three, after natural cooling, wash with pure water several times to obtain the secondary grown lithium iron phosphate.
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A secondary growth preparation method for nano lithium iron phosphate, characterized in that: The steps include: A nano lithium iron phosphate as a seed, a two-dimensional phosphorus element and a reducing agent are subjected to a hydrothermal reaction in a lithium iron phosphate precursor solution; the lithium iron phosphate precursor solution comprises an iron source, a lithium source and a phosphorus source; the reaction temperature of the hydrothermal reaction is 150° C. to 220° C.; and the holding time of the hydrothermal reaction is 150 min to 220 min; The two-dimensional phosphorus element is two-dimensional black phosphorus; the mass ratio of the two-dimensional phosphorus element to the nano-lithium iron phosphate used as a crystal seed is 1:0.4-5; the reducing agent is ascorbic acid; the nano-lithium iron phosphate used as a crystal seed is prepared by a hydrothermal method.
2. The secondary growth preparation method according to claim 1, characterized in that: The iron source is a water-soluble ferrous salt.
3. The secondary growth preparation method according to claim 2, characterized in that: The iron source is ferrous sulfate heptahydrate.
4. The secondary growth preparation method according to claim 1, characterized in that: The lithium source is a water-soluble lithium salt.
5. The secondary growth preparation method according to claim 4, characterized in that: The lithium source is lithium hydroxide monohydrate.
6. The secondary growth preparation method according to claim 1, characterized in that: The phosphorus source is a water-soluble phosphorus source.
7. The secondary growth preparation method according to claim 6, characterized in that: The phosphorus source is phosphoric acid.
8. The secondary growth preparation method according to claim 1, characterized in that: The solvent of the lithium iron phosphate precursor solution is a mixed solvent of water and ethylene glycol.
9. The secondary growth preparation method according to claim 1, characterized in that: The lateral size of the two-dimensional phosphorus single substance is 0.5 μm ~ 100 μm, and the thickness is 1 nm ~ 30 nm.
10. The secondary growth preparation method according to claim 1, characterized in that: In the lithium iron phosphate precursor solution, the molar ratio of iron in the iron source, lithium in the lithium source, and phosphorus in the phosphorus source is 1:3-4:1-2.
11. The secondary growth preparation method according to claim 1, characterized in that: The mass ratio of the reducing agent to the iron source is 1-2:2780.
12. The secondary growth preparation method according to claim 1, characterized in that: The mass ratio of the nano-lithium iron phosphate used as the seed to the iron source is 1-10:
125.
13. The secondary growth preparation method according to claim 1, characterized in that: The secondary growth preparation method also includes post-processing of cooling, washing and drying.
14. The secondary growth preparation method according to claim 1, characterized in that: The particle size of the nano lithium iron phosphate used as the seed crystal is 30 nm to 200 nm.
15. Nano lithium iron phosphate obtained by the secondary growth preparation method according to any one of claims 1 to 14.
16. The use of the nano lithium iron phosphate according to claim 15 in the preparation of lithium ion batteries, characterized in that: Application in the preparation of positive electrode materials for lithium-ion batteries.
Citation Information
Patent Citations
High rate lithium iron phosphate anode material and preparation method thereof
CN102013490A
Preparation method of nanometer lithium iron phosphate positive electrode material and lithium ion battery
CN114171740A
Method for producing lithium iron phosphate by utilizing biomass agent
CN115367724A
Phosphorus-doped carbon coated ultrathin lithium iron phosphate lamellar material and preparation method thereof
CN114583123A
Preparation method of lithium iron phosphate positive electrode material with high tap density and high compaction density
CN115838161A