A method for preparing gold nanoparticle film for refractive index sensing
Through surface coating of star-shaped gold nanoparticles and chemical self-assembly technology, a high-density gold nanoparticle film is prepared, which solves the problems of insufficient sensitivity and response speed of refractive index sensors in the existing technology, and achieves higher transmission. Sensitivity and response speed.
Patent Information
- Application Number
- CN202310273799.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-21
AI Technical Summary
In refractive index sensing, the surface plasmon optical properties of gold nanomaterials cannot be fully utilized in existing technologies, resulting in insufficient sensor sensitivity and response speed.
Star-shaped gold nanoparticles are used as basic nanoparticle units, their surface energy and charge characteristics are changed through surface coating technology, and density-controllable self-assembly deposition is achieved on the surface of transparent substrates through chemical self-assembly technology to prepare high-density nanoparticles. Gold nanoparticle films.
The sensitivity and response speed of the refractive index sensor are improved, a higher density nanoparticle film is formed, and the interaction ability between light and matter is enhanced.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a gold nanoparticle film for refractive index sensing. Background Art
[0002] In recent years, gold nanomaterials have become a research hotspot in nanophotonics and related technologies due to their unique surface plasmon optical properties, such as local field enhancement and strong scattering effects. The surface plasmon optical properties of gold nanomaterials are closely related to the size, shape and structure of the material, as well as the optoelectronic characteristics of the medium environment. Research on the surface plasmon optical properties and applications of gold and silver nanomaterials is one of the important directions in the current field of nano-optics. In the field of sensors, refractive index sensors developed based on the surface plasmon properties of gold nanomaterials have attracted much attention in academia and industry. The refractive index of a material medium is one of the basic physical parameters of a material, which is often related to factors such as material concentration, composition and purity. Gold and silver nanoparticles are coated in different medium environments and show different spectral behaviors. Further analysis of the spectrum can realize timely, convenient and dynamic detection of the composition of the medium material. Compared with traditional electronic sensors, this optical refractive index sensor has the advantages of high sensitivity, fast response speed and small size.
[0003] The present invention adopts Venus star-shaped nanoparticles as basic nanoparticle units. The star-shaped nanoparticles have a sharp branch angle structure and have a stronger surface plasmon effect than nanoparticles of other morphologies. At the same time, through the surface coating technology developed by the present invention, the surface of the nanoparticles is modified to change its surface energy and charge characteristics, and finally density-controlled self-assembly deposition is achieved on the surface of a transparent substrate to obtain a key nanomaterial for refractive index sensing. Summary of the invention
[0004] The present invention aims to solve the problems existing in the prior art and provide a method for preparing a gold nanoparticle film for refractive index sensing.
[0005] The technical solutions adopted in the present invention are:
[0006] A method for preparing a gold nanoparticle film for refractive index sensing, the steps are as follows:
[0007] 1) Prepare gold seed solution;
[0008] 2) HAuCl4 solution and HCl solution are mixed to obtain a growth solution, a gold seed solution is added to the growth solution to obtain a mixed solution, and then AgNO3 solution and ascorbic acid solution are quickly added to the mixed solution at the same time. After stirring for 30 seconds, polyvinyl pyrrolidone (PVP) solution is added to coat the surface of the gold nanostars to obtain a gold nanostar sol;
[0009] 3) Clean the glass substrate and then perform an amination treatment;
[0010] 4) The amino treated glass substrate is placed in the gold nanostar particle sol obtained in step 2) for immersion treatment, and finally a gold nanoparticle film for refractive index sensing is prepared.
[0011] Furthermore, the gold seed solution preparation process in step 1) is as follows:
[0012] In an oil bath at 100°C, 80 mL of 1 mmol / L chloroauric acid solution was heated to complete boiling, and then the heating state was maintained. 12 mL of 1% sodium citrate solution was added during the heating process. After the sodium citrate solution was added, the mixed solution was heated for 15 min and then stopped heating. The reaction bottle was taken out and the mixed solution in the reaction bottle was allowed to cool naturally to room temperature. It was then filtered using a 0.22 µm nitrocellulose membrane to obtain a gold seed solution.
[0013] Furthermore, the sodium citrate solution is stirred by a magnetic stirrer during the process of adding the chloroauric acid solution.
[0014] Furthermore, the growth solution in step 2) is obtained by mixing 2.5 mL of 10 mmol / L HAuCl4 solution and 100 μL of 12 mol / L HCl solution.
[0015] Furthermore, the process of the gold nanostar particle sol in step 2) is as follows:
[0016] At room temperature, after adding 1 mL of gold seed solution to the growth solution, 1 mL of 30 mmol / L AgNO3 solution and 500 µl of 100 mmol / L ascorbic acid (AA) solution were quickly added at the same time. The color of the solution quickly changed from bright yellow to blue-black, and then after continuous stirring for 30 s, the initial sol of gold nanostars was obtained.
[0017] Then, 1 mL of 0.05 mol / L polyvinyl pyrrolidone (PVP) solution was added to the initial gold nanostar sol and stirred continuously until completely mixed. The mixed solution was added with 15 ml of deionized water and placed in a 50 ml centrifuge tube for centrifugation. After centrifugation, the supernatant was poured out and deionized water was added again to redisperse it, finally obtaining the purified gold nanostar particle sol.
[0018] Furthermore, in step 3), the amination treatment process of the glass substrate is as follows:
[0019] After the surface of the glass substrate is cleaned and hydroxylated, the glass substrate is placed in an environment at 70°C for 15 min, then ultrasonically cleaned for 10 min, and finally fully cleaned with deionized water and dried;
[0020] The cleaned and dried glass substrate was immersed in an isopropanol solution containing 2% APTES and 0.1% acetic acid to amino-modify the glass substrate;
[0021] The amination substrate was cleaned with isopropanol and then with deionized water. After cleaning, the glass substrate was annealed in an oven at 120°C for 1 h to complete the amination treatment of the glass substrate.
[0022] Furthermore, the glass substrate is an ITO glass substrate of 0.8*3 cm.
[0023] Furthermore, the glass substrate is cleaned with a Piranha solution, and the surface of the glass substrate is hydroxylated. The Piranha solution is a mixture of 98% H2SO4 and 30% H2O2 in a volume ratio of 7:3.
[0024] Furthermore, in step 4), when the amino-treated IPO glass substrate is immersed in the gold nanostar particle sol, the conductive surface of the glass substrate is placed upward in the gold nanostar particle sol for at least 12 hours. After the immersion is completed, the glass substrate is taken out and placed in an 80°C oven for drying to obtain a dense and uniform gold nanoparticle film for refractive index sensing.
[0025] The present invention has the following beneficial effects:
[0026] The present invention uses star-shaped gold nanoparticles that are more sensitive to the refractive index as the basic core material. Since the star-shaped gold nanoparticles have a high specific surface area and a plurality of sharp-angled branch angle structures, they have a stronger light-matter interaction than nanoparticles of other morphologies, and therefore have a higher refractive index sensing sensitivity.
[0027] The invention utilizes chemical self-assembly technology to realize single-layer deposition of nanoparticles on the surface of a transparent substrate, and the formed nanoparticle film has high density. Implementation
[0028] The present invention provides a method for preparing a gold nanoparticle film for refractive index sensing, comprising the following steps:
[0029] (1) Preparation of gold seeds.
[0030] In an oil bath at 100°C, 80 mL of 1 mmol / L chloroauric acid solution was gradually heated to complete boiling, and then 12 mL of 1% sodium citrate solution was added, and a magnetic stirrer was used to vigorously stir (700 rpm) during the addition process to ensure complete mixing. While keeping the volume of the reaction solution stable, the whole system was kept in a boiling state by continuous heating, and the heating was stopped after 15 min. The reaction bottle was taken out to allow the mixed solution to cool naturally to room temperature, and then filtered using a 0.22 µm nitrocellulose membrane to obtain the gold seed solution required by the present invention and stored in a dark environment at 4°C for a long time for later use.
[0031] (2) Preparation of gold nanostar particle sol
[0032] At room temperature, 2.5 mL of 10 mmol / L HAuCl4 solution and 100 μL of 12 mol / L HCl solution were mixed to obtain a growth solution. Then, 1 mL of gold seed solution was added under moderate stirring (700 rpm) to obtain a mixed solution. 1 ml of 30 mmol / L AgNO3 solution and 500 μl of 100 mmol / L ascorbic acid (AA) solution were quickly added to the mixed solution at the same time. The solution was stirred for reaction. The color of the solution quickly changed from bright yellow to blue-black. After continuous stirring for 30 s, the initial sol of gold nanostars was obtained.
[0033] Then, 1 mL of 0.05 mol / L polyvinyl pyrrolidone (PVP) solution was added to the initial gold nanostar sol and stirred for 20 s to mix them completely. The mixed solution and 15 mL of deionized water were placed in a 50 mL centrifuge tube.
[0034] After the centrifuge tube is weighted, centrifuge it at 4000 RCF for 20 min to prevent nucleation. After centrifugation, pour off the supernatant and add deionized water to redisperse it. For the gold nanostar particles adsorbed on the wall of the centrifuge tube, an ultrasonic cleaner can be used for oscillation, and then stored in a dark environment at 4 °C.
[0035] (3) Amination of glass substrate
[0036] Cut out 0.8*3 cm ITO glass substrates, clean the two cut glass substrates with Piranha solution to hydroxylate the glass surface (Piranha solution is a mixture of 98% H2SO4 and 30% H2O2 in a volume ratio of 7:3), treat at 70 ℃ for 15 min, then ultrasonically clean for 10 min, finally rinse thoroughly with deionized water, and dry in an oven. Soak the treated substrate in an isopropanol solution containing 2% APTES and 0.1% acetic acid. In this experiment, the placement time is 12 h. This step is to fully aminize the substrate. Wash the aminized substrate with isopropanol, then rinse it with deionized water, repeat three times, and anneal the substrate in an oven at 120 ℃ for 1 h after cleaning.
[0037] (4) Self-assembly of gold nanoparticle film
[0038] The annealed substrate was cooled at room temperature. After cooling, the conductive surface of the ITO glass substrate was placed upward into the prepared gold nanoparticle sol for more than 12 hours, and finally placed in an 80°C oven for drying to obtain a dense and uniform gold nanoparticle film for refractive index sensing.
[0039] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.
Claims
1. A method for preparing a gold nanoparticle film for refractive index sensing, Features: Follow these steps: 1) Prepare gold seed solution; 2) HAuCl 4 The solution was mixed with HCl solution to obtain a growth solution, the gold seed solution was added to the growth solution to obtain a mixed solution, and AgNO was quickly added to the mixed solution at the same time. 3 solution and ascorbic acid solution, stirring for reaction, adding polyvinyl pyrrolidone solution to coat the surface of gold nanostar particles, and obtaining gold nanostar particle sol; The process of gold nanostar particle sol is: At room temperature, 1 mL of gold seed solution was added to the growth solution, and 1 mL of 30 mmol / L AgNO was quickly added at the same time. 3 solution and 500 μl of 100 mmol / L ascorbic acid solution, the color of the solution quickly changed from bright yellow to blue-black, and then after continuous stirring for 30 s, the initial sol of gold nanostars was obtained; Then, 1 mL of 0.05 mol / L polyvinyl pyrrolidone solution was added to the initial gold nanostar sol and stirred continuously until completely mixed. The mixed solution was added with 15 mL of deionized water and placed in a 50 mL centrifuge tube for centrifugation. After the centrifugation, the supernatant was poured out and deionized water was added again to redisperse it, and finally the purified gold nanostar particle sol was obtained. 3) Clean the glass substrate and then perform an amination treatment; 4) The amino treated glass substrate is placed in the gold nanostar particle sol obtained in step 2) for immersion treatment, and finally a gold nanoparticle film for refractive index sensing is prepared.
2. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 1, Features: The step 1) of preparing the gold seed solution is as follows: In an oil bath at 100°C, 80 mL of 1 mmol / L chloroauric acid solution was heated to complete boiling, and then the heating state was maintained. 12 mL of 1% sodium citrate solution was added during the heating process. After the sodium citrate solution was added, the mixed solution was heated for 15 min and then stopped heating. The reaction bottle was taken out and the mixed solution in the reaction bottle was allowed to cool naturally to room temperature. It was then filtered using a 0.22 µm nitrocellulose membrane to obtain a gold seed solution.
3. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 2, Features: The sodium citrate solution is stirred by a magnetic stirrer during the process of adding the chloroauric acid solution.
4. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 1, Features: The growth solution in step 2) is 2.5 mL of 10 mmol / L HAuCl 4 The solution was mixed with 100 μL of 12 mol / L HCl solution.
5. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 1, Features: In step 3), the amination treatment process of the glass substrate is as follows: After the surface of the glass substrate is cleaned and hydroxylated, the glass substrate is placed in an environment at 70°C for 15 min, then ultrasonically cleaned for 10 min, and finally fully cleaned with deionized water and dried; The cleaned and dried glass substrate was immersed in an isopropanol solution containing 2% APTES and 0.1% acetic acid to amino-modify the glass substrate; The amination substrate was cleaned with isopropanol and then with deionized water. After cleaning, the glass substrate was annealed in an oven at 120°C for 1 h to complete the amination treatment of the glass substrate.
6. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 5, Features: The glass substrate is an ITO glass substrate of 0.8 cm*3 cm.
7. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 5, Features: The glass substrate is cleaned with a Piranha solution and the surface of the glass substrate is hydroxylated. The Piranha solution is composed of 98% H 2 SO 4 and 30% H 2 O 2 Mix in a 7:3 ratio by volume.
8. The method for preparing the gold nanoparticle film for refractive index sensing according to claim 1, Features: In step 4), when the amino-treated glass substrate is immersed in the gold nanostar particle sol, the conductive surface of the glass substrate is placed upward in the gold nanostar particle sol for at least 12 hours. After the immersion is completed, the glass substrate is taken out and placed in an 80°C oven for drying to obtain a dense and uniform gold nanoparticle film for refractive index sensing.