Single-phase full-spectrum white light fluorescent material and preparation method and application thereof

Through the oxygen vacancies defect luminescence of Ba3MgSi2O8 ceramic material, single-phase full spectrum white light is realized, solving the high cost of rare earth ion luminescence and resource scarcity, and providing low-cost, environmentally friendly and healthy full spectrum white light, suitable for modern lighting needs.

CN116425522BActive Publication Date: 2024-11-08SHENZHEN INSTITUTE OF INFORMATION TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310426473.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-11-08
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Existing full-spectrum white LEDs mainly rely on rare earth ion luminescence, resulting in high costs, low resources and high risk of environmental pollution, and discontinuous spectral effects on lighting quality.

Method used

A single-phase full-spectrum white fluorescent material based on Ba3MgSi2O8 ceramic material is used to achieve full-spectrum white light through oxygen vacancies defect luminescence, avoiding the luminescence of rare earth ion levels. The solid-phase method is used to prepare the process of simple and suitable for industrial production.

Benefits of technology

It has achieved a full-spectrum white light emission with low cost, rich resources, high color rendering index, and environmentally friendly and healthy full-spectrum white light emission, which is suitable for modern healthy lighting needs, solves the limitations of rare earth ion luminescence, and improves spectral continuity and lighting quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116425522B_ABST
    Figure CN116425522B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of fluorescent materials, and in particular to a single-phase full-spectrum white light fluorescent material and a preparation method and application thereof. The single-phase full-spectrum white light fluorescent material is a Ba3MgSi2O8 ceramic material. The Ba3MgSi2O8 fluorescent ceramic of the present invention is a single-phase full-spectrum white light fluorescent material, and the luminescence mainly comes from oxygen vacancy defect luminescence, non-rare earth ion energy level transition luminescence, low cost, and solves the problem that the existing full-spectrum white light mainly comes from the limitation of rare earth ion luminescence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fluorescent materials, and in particular to a single-phase full-spectrum white light fluorescent material and a preparation method and application thereof. Background Art

[0002] With the accelerated development of white light LEDs in the field of lighting, the market has higher and higher requirements for the quality of white light LED light sources. From the initial pursuit of brightness and power conversion, to the current composite light source that combines light efficiency, color reproduction, color temperature, quality and health, and finally to the pursuit of full-spectrum lighting that is close to sunlight, high-quality lighting is the future development trend. At present, the fluorescent conversion materials used for full-spectrum LEDs include mixed phosphor systems and single-matrix fluorescent material systems. The mixed phosphor system mixes phosphors that emit different colors of fluorescence together to achieve full-spectrum emission through various color combinations. However, the mixed phosphor system is inevitably affected by the matching and physical and chemical properties of the phosphors, as well as the low light efficiency caused by the mutual absorption between colors, which affects the light quality of the LED light source.

[0003] Therefore, it is very important to develop single-phase full-spectrum emission fluorescent materials. In recent years, researchers have made a lot of progress in single-phase full-spectrum white light luminescent materials. Common research methods include ion co-doping, ion doping and energy transfer. Ion co-doping refers to the simultaneous doping of different ions into the material, and the use of the difference in their energy level structure to achieve full-spectrum luminescence. For example, by co-doping erbium, neodymium and other ions in the phosphor, a full-spectrum luminescence effect can be achieved. Ion doping refers to the doping of a small amount of a certain ion into the material to change the energy band structure of the material, thereby achieving full-spectrum luminescence. For example, doping indium oxide into the phosphor can achieve a full-spectrum luminescence effect. Energy transfer refers to the transfer of energy in the material from one ion to another to achieve full-spectrum luminescence. For example, the energy transfer effect of cadmium sulfide and zinc sulfide can be used to achieve full-spectrum luminescence. It can be found that most of the existing full-spectrum white light is achieved by single or multiple doping of rare earth ions. As a non-renewable resource, rare earth ions have the characteristics of high cost, fixed luminescence peak position and environmental pollution.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a single-phase full-spectrum white light fluorescent material, which is based on the luminescence of oxygen vacancy defects in the material rather than rare earth energy level luminescence.

[0006] Another object of the present invention is to provide a method for preparing a single-phase full-spectrum white light fluorescent material.

[0007] Another object of the present invention is to provide application of a single-phase full-spectrum white light fluorescent material in a full-spectrum white light LED.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] Single-phase full-spectrum white light fluorescent material, which is Ba3MgSi2O8 ceramic material.

[0010] The single-phase full-spectrum white light fluorescent material of the present invention does not dope the Ba3MgSi2O8 material, but emits light based on the oxygen vacancy defects of the Ba3MgSi2O8 material, thus overcoming the limitation that the existing full-spectrum white light mainly comes from the emission of rare earth ions.

[0011] In a specific embodiment of the present invention, the single-phase full-spectrum white light fluorescent material emits full-spectrum white light with a spectral range covering the entire visible light band of 400 to 700 nm under the excitation of ultraviolet light.

[0012] In a specific embodiment of the present invention, the chromaticity coordinates CIE of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light are (0.365-0.385, 0.315-0.395), such as (0.375, 0.360).

[0013] In a specific embodiment of the present invention, the color temperature of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light is 3858-4226K, such as 4043K.

[0014] In a specific embodiment of the present invention, the excitation wavelength of the ultraviolet light is 255-365 nm.

[0015] The present invention also provides a method for preparing any one of the above-mentioned single-phase full-spectrum white light fluorescent materials, comprising the following steps:

[0016] Ba, Mg and Si are weighed in a molar ratio of 1:(0.9-1.1):(0.9-1.1) respectively, and mixed with an auxiliary agent to obtain a mixed material, and then calcined, tableted and sintered;

[0017] During the sintering treatment, the sintering is carried out in a reducing atmosphere for 8 to 16 hours.

[0018] In a specific embodiment of the present invention, the reducing atmosphere includes hydrogen and nitrogen. Further, in the reducing atmosphere, the volume fraction of hydrogen is 5%.

[0019] In a specific embodiment of the present invention, the sintering temperature is 1200-1400°C.

[0020] In a specific embodiment of the present invention, the Ba source, Mg source and Si source are BaCO3, MgO and SiO2 respectively.

[0021] In a specific embodiment of the present invention, the auxiliary agent includes at least one of a dispersant, a binder and a sintering aid.

[0022] In a specific embodiment of the present invention, the calcination conditions include: the calcination temperature is 800-1000° C., and the calcination time is 2-6 hours.

[0023] In a specific embodiment of the present invention, the tabletting conditions include: pre-pressing into a green blank, and then cold isostatic pressing for 60 to 240 seconds at 200 to 280 MPa.

[0024] The present invention also provides application of any one of the above-mentioned single-phase full-spectrum white light fluorescent materials in the field of full-spectrum white light LEDs.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The Ba3MgSi2O8 fluorescent ceramic of the present invention is a single-phase full-spectrum white light fluorescent material, and the luminescence mainly comes from oxygen vacancy defects, not rare earth ion energy level transition luminescence, and has low cost, solving the limitation problem that the existing full-spectrum white light mainly comes from rare earth ion luminescence;

[0027] (2) The present invention adopts a solid phase method to prepare a single-phase full-spectrum white light fluorescent material, which has a simple preparation process, a short cycle, simple and cheap raw materials, and is conducive to industrial large-scale production;

[0028] (3) The Ba3MgSi2O8 fluorescent ceramic of the present invention can obtain full-spectrum white light covering the entire visible light band of 400-700nm through 255-365nm ultraviolet light excitation, which is more suitable for the needs of modern healthy lighting and has broad application prospects in the field of white light LEDs. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The X-ray diffraction pattern of Ba3MgSi2O8 provided in Example 1 of the present invention;

[0031] Figure 2 X-ray diffraction pattern of BaMgSiO4 provided for Comparative Example 1;

[0032] Figure 3The emission spectrum of Ba3MgSi2O8 under 332nm excitation provided in Example 1 of the present invention;

[0033] Figure 4 The emission spectrum of BaMgSiO4 provided in Comparative Example 1 under 332nm excitation;

[0034] Figure 5 This is a physical picture of Ba3MgSi2O8 provided in Example 1 of the present invention under 332nm excitation;

[0035] Figure 6 A physical image of BaMgSiO4 provided in Comparative Example 1 under 332nm excitation;

[0036] Figure 7 The chromaticity coordinate diagram of Ba3MgSi2O8 under 332nm excitation provided in Example 1 of the present invention;

[0037] Figure 8 The emission spectrum of Ba3MgSi2O8 under 327nm excitation provided by Example 1 of the present invention;

[0038] Fig. 9 This is a physical picture of Ba3MgSi2O8 provided in Example 1 of the present invention under 327nm excitation;

[0039] Fig.10 This is a chromaticity coordinate diagram of Ba3MgSi2O8 provided in Example 1 of the present invention under 327nm excitation. DETAILED DESCRIPTION

[0040] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0041] At present, the main methods for realizing white light LED include:

[0042] (1) The blue light chip is used to excite the yellow fluorescence to emit yellow light, and the blue light is then combined with the yellow light to form white light;

[0043] (2) Use the purple light chip to excite the three-primary color phosphors to emit white light;

[0044] (3) Use the purple light chip to excite the single-matrix full-color phosphor to emit white light;

[0045] Among them, the first method lacks the red light part, resulting in a low color rendering index of the white light LED, low luminous efficiency, and uneven color temperature spatial distribution. The second method has a great impact on the lumen efficiency and color reproduction because the white light synthesized by the three primary colors often has problems with mutual color absorption and ratio control after the phosphors are mixed. The third method can overcome the above problems and is a better solution for LED to achieve white light.

[0046] In addition, methods (1) and (2) will produce an excessively high blue light peak near 450nm, which will disrupt the normal circadian rhythm; too much blue light is also easily scattered in the human eye, resulting in a decrease in the overall contrast ratio and causing glare. Full-spectrum white light can achieve a natural and realistic lighting environment, making the effect of objects more realistic; it can regulate the human physiological rhythm and eliminate the harm of blue light. In order for white light to obtain excellent color rendering, it is necessary to make every effort to simulate daylight, that is, the spectrum must be continuous throughout the visible light range, from deep blue to deep red.

[0047] Single-phase full-spectrum white light fluorescent material, which is Ba3MgSi2O8 ceramic material.

[0048] The single-phase full-spectrum white light fluorescent material of the present invention does not dope the Ba3MgSi2O8 material, but emits light based on the oxygen vacancy defects of the Ba3MgSi2O8 material, thus overcoming the limitation that the existing full-spectrum white light mainly comes from the emission of rare earth ions.

[0049] The single-phase full-spectrum white light fluorescent material of the present invention is a full-spectrum white light luminescent material that emits light at non-rare earth energy levels. Compared with rare earth luminescent materials, it has the advantages of low cost, abundant resources, high color rendering index, full-spectrum luminescence, environmental protection and health, as follows:

[0050] Low cost: Because the price of rare earth elements is relatively high, the cost of the Ba3MgSi2O8 ceramic material of the present invention, which is a non-rare earth doped non-rare earth level luminescent material, is lower than that of rare earth luminescent materials;

[0051] Rich resources: The elements corresponding to the non-rare earth energy level luminescent materials of the present invention are common elements, and the resources are more abundant than rare earth elements. Therefore, the non-rare earth energy level luminescent materials have a wider application prospect;

[0052] High color rendering index: The non-rare earth energy level luminescent material of the present invention has a high color rendering index, which can restore the color of the object more realistically, making it have better effects in lighting, display, etc.;

[0053] Full spectrum luminescence: The non-rare earth energy level luminescent material of the present invention can emit a continuous and smooth spectrum, so that it can produce more real white light and better meet people's demand for white light quality;

[0054] Environmental protection and health: Since the mining and processing of rare earth elements may cause environmental pollution and damage to human health, the non-rare earth energy level luminescent material of the present invention is more environmentally friendly and healthy than rare earth luminescent materials.

[0055] In a specific embodiment of the present invention, the single-phase full-spectrum white light fluorescent material emits full-spectrum white light with a spectral range covering the entire visible light band of 400 to 700 nm under the excitation of ultraviolet light.

[0056] The single-phase full-spectrum white light material of the present invention can generate light emission mainly based on oxygen vacancy defects under the excitation of ultraviolet light, and the spectrum covers the entire visible light band.

[0057] In a specific embodiment of the present invention, the chromaticity coordinates CIE of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light are (0.365-0.385, 0.315-0.395), such as (0.375, 0.360).

[0058] In a specific embodiment of the present invention, the color temperature of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light is 3858-4226K, such as 4043K.

[0059] In a specific embodiment of the present invention, the excitation wavelength of the ultraviolet light is 255-365 nm.

[0060] For example, in different embodiments, the excitation wavelength of the ultraviolet light can be 255 nm, 265 nm, 275 nm, 285 nm, 295 nm, 305 nm, 315 nm, 325 nm, 335 nm, 345 nm, 355 nm, 365 nm, or a range consisting of any two of them.

[0061] The present invention also provides a method for preparing any one of the above-mentioned single-phase full-spectrum white light fluorescent materials, comprising the following steps:

[0062] Ba, Mg and Si are weighed in a molar ratio of 1:(0.9-1.1):(0.9-1.1) respectively, and mixed with an auxiliary agent to obtain a mixed material, and then calcined, tableted and sintered;

[0063] During the sintering treatment, the sintering is carried out in a reducing atmosphere for 8 to 16 hours.

[0064] For example, in different embodiments, in the sintering treatment, the treatment time under a reducing atmosphere can be 8 h, 8.5 h, 9 h, 9.5 h, 10 h, 10.5 h, 11 h, 11.5 h, 12 h, 13 h, 14 h, 15 h, 16 h or a range consisting of any two of them.

[0065] For example, in different embodiments, the molar ratio of the Ba source and the Mg source, calculated as Ba and Mg respectively, can be 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1 or a range consisting of any two of them; the molar ratio of the Ba source and the Si source, calculated as Ba and Si respectively, can be 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1 or a range consisting of any two of them; the molar ratio of the Mg source and the Si source, calculated as Mg and Si respectively, can be 1:1, 0.9:0.95, 0.9:1, 0.9:1.05, 0.9:1.1, 1:0.9, 1:1.1, 1.1:0.9, 1.1:1 or a range consisting of any two of them.

[0066] In a specific embodiment of the present invention, the molar ratio of the Ba source, the Mg source and the Si source, calculated as Ba, Mg and Si respectively, is 1:1:1.

[0067] The present invention adopts the preparation method to form a large number of oxygen vacancies during the high-temperature synthesis process in a reducing atmosphere, and utilizes the formed oxygen vacancy defect transition luminescence to obtain a single-phase full-spectrum white light fluorescent material.

[0068] In a specific embodiment of the present invention, the reducing atmosphere includes hydrogen and nitrogen. Further, in the reducing atmosphere, the volume fraction of hydrogen is 5%.

[0069] In a specific embodiment of the present invention, the sintering temperature is 1200-1400°C.

[0070] For example, in different embodiments, the sintering temperature may be 1200°C, 1220°C, 1250°C, 1280°C, 1300°C, 1320°C, 1350°C, 1380°C, 1400°C or a range consisting of any two of them.

[0071] In actual operation, the sintering treatment can be carried out in a tube furnace. The sheet obtained after tableting is placed in a tube furnace, and 5% nitrogen and hydrogen mixed gas is introduced to sinter at 1200-1400° C. for 8-12 hours, and then taken out after cooling to room temperature after sintering.

[0072] In a specific embodiment of the present invention, the Ba source, Mg source and Si source are BaCO3, MgO and SiO2 respectively.

[0073] In a specific embodiment of the present invention, the auxiliary agent includes at least one of a dispersant, a binder and a sintering aid.

[0074] In actual operation, the types of dispersants, binders and sintering aids in the additives can be adjusted and selected according to actual needs, as long as the corresponding conventional effects can be achieved; the dispersant ensures the uniformity of raw material dispersion and avoids agglomeration; the binder ensures the composite molding of the raw materials during the ball milling process; the sintering aid improves the density of the product during the sintering process.

[0075] For example, the dispersant may be at least one of fish oil, oleic acid, triethyl phosphate and polyethylene glycol; the binder may be at least one of polyvinyl butyral, polyvinyl alcohol and ethyl cellulose; the sintering aid may be at least one of tetraethyl orthosilicate, magnesium oxide, yttrium trioxide, yttrium fluoride, calcium fluoride, calcium carbonate, lithium carbonate, silicon dioxide and boric acid. The mass of the dispersant is 0.5% to 1% of the total mass of the Ba source, Mg source and Si source; the mass of the binder is 0.5% to 5% of the total mass of the Ba source, Mg source and Si source; the mass of the sintering aid is 0.1% to 0.5% of the total mass of the Ba source, Mg source and Si source.

[0076] In a specific embodiment of the present invention, the mixing method includes ball milling. Further, the ball milling medium used in the ball milling is zirconium dioxide; the dispersing solvent used in the ball milling is ethanol. Further, the ball milling time is 12 to 24 hours.

[0077] For example, in different embodiments, the ball milling time can be 12h, 14h, 15h, 16h, 18h, 20h, 22h, 24h or a range consisting of any two thereof. The specific ball milling time can be adjusted according to the situation to ensure uniform mixing of the materials.

[0078] In actual operation, during the ball milling process, the mass ratio of the dispersing solvent to the mixed material can be (1-1.2):1; during the ball milling process, the ball-to-material ratio can be controlled at 1:3.

[0079] In actual operation, the ball-milled slurry is dried, crushed by grinding or the like to obtain a powder, and then calcined. The drying can be performed in a conventional oven or other equipment.

[0080] In a specific embodiment of the present invention, the calcination conditions include: the calcination temperature is 800-1000° C., and the calcination time is 2-6 hours.

[0081] For example, in different embodiments, the calcination temperature can be 800°C, 820°C, 850°C, 880°C, 900°C, 920°C, 950°C, 980°C, 1000°C or a range consisting of any two thereof; the calcination time can be 2h, 3h, 4h, 5h, 6h or a range consisting of any two thereof.

[0082] In actual operation, the calcination can be carried out in a box furnace. Further, after the calcination, the calcined material is ground and sieved, and the powder with a particle size of less than 150 μm is taken for tableting.

[0083] In a specific embodiment of the present invention, the tabletting conditions include: pre-pressing into a green blank, and then cold isostatic pressing for 60 to 240 seconds at 200 to 280 MPa.

[0084] In actual operation, the pre-pressing may be performed by dry pressing, and the specific pre-pressing pressure may be 3-20 MPa.

[0085] The present invention also provides application of any one of the above-mentioned single-phase full-spectrum white light fluorescent materials in the field of full-spectrum white light LEDs.

[0086] The single-phase full-spectrum white light fluorescent material of the present invention is a full-spectrum luminescent material that emits light at non-rare earth energy levels and has broad application prospects in the fields of lighting, display, biomedicine, etc.

[0087] Example 1

[0088] This embodiment provides a method for preparing a single-phase full-spectrum white light fluorescent material Ba3MgSi2O8, comprising the following steps:

[0089] (1) BaCO3, MgO and SiO2 were weighed according to a stoichiometric ratio (the molar ratio of Ba, Mg and Si was 1:1:1), and then oleic acid was added to obtain a mixed material; ethanol was added to the mixed material, and then zirconium oxide balls were added at a ball-to-material ratio of 1:3, and the mixture was placed in a ball mill and subjected to bidirectional ball milling for 24 hours to obtain a mixed slurry;

[0090] The mass of oleic acid is 1% of the total mass of BaCO3, MgO and SiO2, and the mass of ethanol is 1 times the mass of the mixed material.

[0091] (2) The mixed slurry obtained in step (1) was transferred to a glass dish and dried in an oven at 50° C.; the dried powder was ground in an agate mortar and then calcined in a box furnace at 900° C. in an air atmosphere for 4 h.

[0092] (3) The powder calcined in step (2) is taken out, ground, sieved, and the powder with a particle size of less than 150 μm is pressed into tablets; the tableting comprises: pre-pressing the powder with a particle size of less than 150 μm into thin sheets using a dry press at a pressure of 5 MPa, wrapping it and placing it in a cold isostatic press, and cold isostatically pressing it at a pressure of 240 MPa for 2 minutes to obtain a formed sheet.

[0093] (4) The sheet obtained in step (3) is placed in a tubular furnace, a 5% nitrogen-hydrogen mixed gas is introduced, and sintered at 1300° C. for 16 h. After cooling to room temperature, the sheet is taken out to obtain a single-phase full-spectrum white light fluorescent material Ba3MgSi2O8.

[0094] Example 2

[0095] This example is prepared by referring to the method of Example 1, with the only difference being that the sintering conditions in step (4) are different.

[0096] In this embodiment, the sintering temperature of step (4) is 1300° C. and the sintering time is 8 hours.

[0097] Example 3

[0098] This example is prepared by referring to the method of Example 1, with the only difference being that the sintering conditions in step (4) are different.

[0099] In this embodiment, the sintering temperature of step (4) is 1300° C. and the sintering time is 10 h.

[0100] Example 4

[0101] This example is prepared by referring to the method of Example 1, with the only difference being that the sintering conditions in step (4) are different.

[0102] In this embodiment, the sintering temperature of step (4) is 1200° C. and the sintering time is 16 hours.

[0103] Example 5

[0104] This example is prepared by referring to the method of Example 1, with the only difference being that the sintering conditions in step (4) are different.

[0105] In this embodiment, the sintering temperature of step (4) is 1400° C. and the sintering time is 16 hours.

[0106] Comparative Example 1

[0107] Comparative Example 1 provides a method for preparing the fluorescent material BaMgSiO4, referring to Example 1, except that the sintering atmosphere in step (4) is air and the sintering time is 2 hours.

[0108] Experimental Example 1

[0109] Figure 1This is the X-ray diffraction pattern of Ba3MgSi2O8 prepared in Example 1 of the present invention. Figure 2 This is the X-ray diffraction pattern of BaMgSiO4 prepared in Comparative Example 1.

[0110] Figure 3 This is the emission spectrum of Ba3MgSi2O8 under 332nm ultraviolet light excitation provided in Example 1 of the present invention. As can be seen from the figure, the emission peak range of Ba3MgSi2O8 covers the full spectrum white light of the entire visible light band of 400-700nm. Figure 4 The emission spectrum of BaMgSiO4 prepared in Comparative Example 1 under 332nm ultraviolet light excitation is shown in the figure. As can be seen from the figure, the emission peak of BaMgSiO4 is in the blue and purple light range.

[0111] Figure 5 This is a physical picture of Ba3MgSi2O8 under 332nm ultraviolet light excitation provided in Example 1 of the present invention. From the picture, the generation of white light can be clearly observed. Figure 6 This is a real picture of BaMgSiO4 under 332nm excitation provided for Comparative Example 1. From the picture, the generation of blue light can be observed.

[0112] Figure 7 The chromaticity coordinate diagram of Ba3MgSi2O8 provided in Example 1 of the present invention under 332nm ultraviolet light excitation is (0.375, 0.360), and the color temperature is 4043K.

[0113] Figure 8 This is the emission spectrum of Ba3MgSi2O8 under 327nm ultraviolet light excitation provided in Example 1 of the present invention. As can be seen from the figure, the emission peak range of Ba3MgSi2O8 covers the full spectrum white light of the entire visible light band of 400-700nm.

[0114] Fig. 9 This is a physical picture of Ba3MgSi2O8 under 327nm ultraviolet light excitation provided in Example 1 of the present invention. From the picture, the generation of white light can be clearly observed.

[0115] Fig.10 The chromaticity coordinate diagram of Ba3MgSi2O8 provided in Example 1 of the present invention under 327nm ultraviolet light excitation is (0.369, 0.317), and the color temperature is 3866K.

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. Single-phase full-spectrum white light fluorescent material, characterized in that: It is Ba3MgSi2O8 ceramic material; The single-phase full-spectrum white light fluorescent material emits full-spectrum white light covering the entire visible light band of 400 to 700 nm under the excitation of ultraviolet light of 255 to 365 nm; The preparation method of the Ba3MgSi2O8 ceramic material is as follows: Ba source, Mg source and Si source are weighed in a molar ratio of 1:(0.9-1.1):(0.9-1.1) respectively, mixed with an additive to obtain a mixed material, and calcined, tableted and sintered; the calcination conditions include: the calcination temperature is 800-1000°C, the calcination time is 2-6h, and the calcination atmosphere is an air atmosphere; in the sintering treatment, the sintering temperature is 1300-1400°C, and the treatment is carried out in a reducing atmosphere for 16h.

2. The single-phase full-spectrum white light fluorescent material according to claim 1, characterized in that: The chromaticity coordinates CIE of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light are (0.365-0.385, 0.315-0.395).

3. The single-phase full-spectrum white light fluorescent material according to claim 1, characterized in that: The color temperature of the single-phase full-spectrum white light fluorescent material under the excitation of ultraviolet light is 3858-4226K.

4. The single-phase full-spectrum white light fluorescent material according to any one of claims 2 to 3, characterized in that: The excitation wavelength of the ultraviolet light is 255-365 nm.

5. The single-phase full-spectrum white light fluorescent material according to claim 1, characterized in that: The reducing atmosphere includes hydrogen and nitrogen.

6. The single-phase full-spectrum white light fluorescent material according to claim 5, characterized in that: In the reducing atmosphere, the volume fraction of the hydrogen is 5%.