A high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting and its preparation method
By introducing SrAl2O4 as the second phase into Ce:LuAG ceramics, a complex-phase fluorescent ceramic with high brightness and high luminous efficiency is prepared, which solves the problems of poor thermal stability and low light conversion efficiency of Ce:LuAG ceramics and achieves a lower sintering temperature. and higher light extraction rate, suitable for high-power LEDs/LDs devices.
Patent Information
- Application Number
- CN202310434299.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Due to its cubic crystal structure, Ce:LuAG transparent ceramic phosphor has problems of poor thermal stability and low light conversion efficiency, and its high sintering temperature limits its large-scale application.
The second phase SrAl2O4 is introduced into the ceramic matrix, and Ce:YAG composite phase fluorescent ceramics are prepared through discharge plasma sintering, which improves the uniformity of emitted light and light extraction efficiency and reduces the sintering temperature.
It significantly improves the thermal stability and light conversion efficiency of fluorescent ceramics, reduces preparation costs, is suitable for high-power LEDs/LDs devices, and enhances the application value of the device.
Smart Images

Figure CN116425544B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorescent ceramics, and in particular relates to a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting and a preparation method thereof. Background Art
[0002] LuAG is the abbreviation of lutetium aluminum garnet, and its chemical formula is Lu 3 Al 5 O 12 , is by Lu 2 O 3 and Al 2 O 3 The solid solution formed belongs to the cubic crystal system and has a garnet structure. It does not have a birefringence effect and can be made into transparent ceramics with excellent optical properties. At the same time, due to the high density (6.73g / cm 3 , equivalent to 94% of the density of BGO), high melting point (2010℃), high effective atomic number (Z eff =60), good mechanical properties, and can maintain stable optical and physical and chemical properties under long-term radiation conditions.
[0003] Ce:LuAG transparent ceramic phosphor has been widely studied as a promising candidate material for color converters for white light-emitting diode (LED) lighting due to its excellent thermal and chemical stability. The Shanghai Institute of Silicates used a solid-phase reaction method to prepare transparent LuAG:Ce ceramics under vacuum sintering conditions at 1760°C for 10 hours. The transmittance is low, which is 56% in the visible light range. In addition, the high sintering temperature of 1760°C also limits its large-scale application. Patent CN110550945 B discloses a method for preparing LuAG:Ce transparent ceramics and LuAG:Ce transparent ceramics, which can solve the problems of low transmittance of LuAG:Ce ceramics in the visible light range in the prior art and the limitation of large-scale application due to high sintering temperature during preparation.
[0004] However, Ce:LuAG transparent ceramic phosphor has a cubic crystal structure, and although it has a high transmittance, it also causes the blue light emitted by the InGaN chip to 3+ It has less absorption, lower yellow light conversion efficiency, and has problems of poor thermal stability and low light conversion efficiency. Summary of the invention
[0005] In view of the above-mentioned technical deficiencies, the purpose of the present invention is to provide a high-brightness and high-luminous-efficiency complex phase fluorescent ceramic for laser lighting and a preparation method thereof. The fluorescent ceramic has better luminous characteristics, solves the problems of poor thermal stability and low light conversion efficiency in the prior art. The preparation method of the complex phase ceramic is simple, time-saving and low-sintering temperature, and can be applied to high-power LEDs / LDs devices, greatly improving the application value of the device.
[0006] In order to solve the above problems, a second phase is introduced into the ceramic matrix to control its light transmittance and enhance the optical path. 2 O 4 As the second phase to prepare Ce:YAG composite fluorescent ceramics, SrAl 2 O 4 The introduction of can significantly improve the uniformity of the emitted light of the complex phase fluorescent ceramics, making it more suitable for white light laser diode illumination.
[0007] SrAl 2 O 4 As a widely used traditional ceramic, it has attracted extensive attention due to its unique properties. 2 O 3 In comparison, SrAl 2 O 4 It belongs to the hexagonal system and has a lower refractive index, which helps to reduce total reflection loss and improve light extraction efficiency. 2 O 4 The vacuum sintering temperature is the same as Ce:LuAG, which is convenient for preparing SrAl in one step vacuum sintering. 2 O 4 -Ce:LuAG.
[0008] The specific technical solution adopted by the present invention is as follows:
[0009] The first object of the present invention is to provide a high brightness and high luminous efficiency composite fluorescent ceramic for laser lighting, wherein the composite fluorescent ceramic is Ce: LuAG powder, SrAl 2 O 4 The powder is used as a ceramic raw material powder and is prepared by spark plasma sintering, in which Ce:LuAG is used as the ceramic main body and SrAl is introduced 2 O 4 It is the second phase, and the prepared composite fluorescent ceramic has high brightness and high luminous efficiency.
[0010] The second object of the present invention is to provide a method for preparing a high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting, comprising the following steps:
[0011] S1: Weigh Ce:LuAG powder, SrAl 2 O4 Powder, as ceramic raw material powder, SrAl 2 O 4 The powder accounts for 5% to 25% of the total mass of the ceramic raw material powder;
[0012] S2: Ce:LuAG powder and SrAl 2 O 4 After the powders are blended, anhydrous ethanol is added and the mixture is fully mixed by ball milling;
[0013] S3: taking out the slurry obtained after ball milling and drying it to obtain dry powder;
[0014] S4: The dried powder is subjected to spark plasma sintering in a vacuum state, and then cooled to room temperature to obtain a composite fluorescent ceramic.
[0015] Furthermore, in step S1, the particle size of the Ce:LuAG powder is 1 μm to 1.3 μm, and the particle size of the SrAl 2 O 4 The particle size of the powder is 1.5μm to 2μm, and the purity is above 99.99%.
[0016] Furthermore, in step S2, the ball milling speed is 180-250 rpm, and the ball milling time is 15-30 h.
[0017] Furthermore, in step S3, the drying temperature is 70-90° C., and the drying time is 8-12 hours.
[0018] Furthermore, in step S4, the sintering pressure of the spark plasma sintering is 50-100 MPa, the pulse current is 200-400 A, the heat preservation sintering time is 20-50 min, and the sintering temperature is 1650° C.-1800° C.
[0019] The beneficial effects of the present invention are:
[0020] 1. SrAl used in the present invention 2 O 4 The vacuum sintering temperature is the same as Ce:LuAG, which is convenient for one-step vacuum sintering, lower cost and more environmentally friendly;
[0021] 2. The present invention adopts SrAl 2 O 4 -Ce:LuAG complex phase, through SrAl 2 O 4 The introduction of the second phase significantly inhibits the grain growth of LuAG, making the Ce:LuAG particles small and uniform, effectively improving the light extraction rate;
[0022] 3. SrAl prepared by the present invention 2 O 4-Ce:LuAG composite phase, with high thermal stability and low thermal quenching rate (92% @ 150 ℃); compared with pure Ce:LuAG fluorescent ceramics, it has better luminescence characteristics. Under the excitation of 20W blue light LD chip, there is no luminescence saturation, especially when the input power is 4-5W, 20wt% SrAl 2 O 4 -Ce:LuAG's maximum luminous flux can reach 800-1000lm, greatly improving the application value of the device.
[0023] 4. The present invention prepares SrAl with high brightness and high luminous efficiency by SPS sintering 2 O 4 -Ce:LuAG composite ceramics have a simple preparation method, short time and low sintering temperature, and can be used in high-power LEDs / LDs devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 The sample SrAl prepared in Example 2 of the present invention 2 O 4 -Ce:LuAG and LuAG, SrAl 2 O 4 XRD comparison diagram of
[0026] Figure 2 The sample SrAl prepared in Example 2 of the present invention 2 O 4 -EL spectrum of Ce:LuAG under 450nm LD chip excitation;
[0027] Figure 3 The SrAl prepared in Example 1 of the present invention 2 O 4 Comparison of the relationship between the luminous flux and the LD chip input power of the sample accounting for 25% of the total mass of the ceramic raw materials, the 20% sample prepared in Example 2, and the pure Ce:LuAG sample. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Ce:LuAG powder, SrAl 2 O 4 The powders are all commercially available products.
[0030] Example 1
[0031] According to the chemical formula SrAl 2 O 4 -Ce:SrAl in LuAG 2 O 4 According to the stoichiometric ratio of the corresponding raw materials, 60 g of Ce:LuAG powder with a purity of 99.99% and a particle size of 1.2 μm, 60 g of SrAl with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively. 2 O 4 Powder 15g. Ce:LuAG powder and SrAl 2 O 4 After the powders are blended, anhydrous ethanol is added and the mixture is thoroughly mixed by ball milling. The powder obtained after ball milling is dried in an oven at 90°C for 12 hours to obtain dry powder. The dry powder is wrapped with graphite paper and then subjected to spark plasma sintering under vacuum. The sintering pressure is 80 MPa, the pulse current is 300 A, the heat preservation sintering time is 40 min, the sintering temperature is 1700°C, and the composite ceramics are obtained after cooling to room temperature.
[0032] Under the excitation of the blue light LD chip with a wavelength of about 450nm, it emits high-brightness broadband yellow light near 540nm. Compared with pure Ce:LuAG, it exhibits excellent luminescence performance under the excitation of blue light LD. When the input power is 4.5W, 25wt% SrAl 2 O 4 -Ce:LuAG reaches a maximum luminous flux of 800lm.
[0033] Example 2
[0034] According to the chemical formula SrAl 2 O 4 -Ce:SrAl in LuAG 2 O 4According to the stoichiometric ratio of the corresponding raw materials, 60 g of Ce:LuAG powder with a purity of 99.99% and a particle size of 1.2 μm, 60 g of SrAl with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively. 2 O 4 Powder 12g. Ce:LuAG powder and SrAl 2 O 4 After the powders are blended, anhydrous ethanol is added and the mixture is thoroughly mixed by ball milling. The powder obtained after ball milling is dried in an oven at 90°C for 12 hours to obtain dry powder. The dry powder is wrapped with graphite paper and then subjected to spark plasma sintering under vacuum. The sintering pressure is 80 MPa, the pulse current is 300 A, the heat preservation sintering time is 40 min, the sintering temperature is 1700°C, and the composite ceramics are obtained after cooling to room temperature.
[0035] Under the excitation of the blue light LD chip with a wavelength of about 450nm, a high-brightness broadband yellow light is emitted near 540nm. When the input power is 5W, 20wt% SrAl 2 O 4 -Ce:LuAG does not show luminous saturation and the luminous flux can reach 1000lm.
[0036] Example 3
[0037] According to the chemical formula SrAl 2 O 4 -Ce:SrAl in LuAG 2 O 4 According to the stoichiometric ratio of the corresponding raw materials, 60 g of Ce:LuAG with a purity of 99.99% and a particle size of 1.2 μm, 60 g of SrAl with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively, accounting for 10% of the total mass of the ceramic raw materials. 2 O 4 6g of powder. Mix Ce:LuAG powder with SrAl 2 O 4 After the powders are blended, anhydrous ethanol is added and the mixture is thoroughly mixed by ball milling. The powder obtained after ball milling is dried in an oven at 90°C for 12 hours to obtain dry powder. The dry powder is wrapped with graphite paper and then subjected to spark plasma sintering under vacuum. The sintering pressure is 80 MPa, the pulse current is 300 A, the heat preservation sintering time is 40 min, the sintering temperature is 1700°C, and the composite ceramics are obtained after cooling to room temperature.
[0038] When excited by a blue light LD chip with a wavelength of about 450nm, it emits high-brightness broadband yellow light at about 540nm. When the input power is 3.3W, 10wt% SrAl 2 O 4 -Ce:LuAG reaches a maximum luminous flux of 600lm.
[0039] Example 4
[0040] According to the chemical formula SrAl 2 O 4 -Ce:SrAl in LuAG 2 O 4 According to the stoichiometric ratio of the corresponding raw materials, 60 g of Ce:LuAG with a purity of 99.99% and a particle size of 1.2 μm, 60 g of SrAl with a purity of 99.99% and a particle size of 1.7 μm were weighed respectively, accounting for 5% of the total mass of the ceramic raw materials. 2 O 4 3g of powder. Mix Ce:LuAG powder with SrAl 2 O 4 After the powders are blended, anhydrous ethanol is added and the mixture is thoroughly mixed by ball milling. The powder obtained after ball milling is dried in an oven at 90°C for 12 hours to obtain dry powder. The dry powder is wrapped with graphite paper and then subjected to spark plasma sintering under vacuum. The sintering pressure is 80 MPa, the pulse current is 300 A, the heat preservation sintering time is 40 min, the sintering temperature is 1700°C, and the composite ceramics are obtained after cooling to room temperature.
[0041] When excited by a blue light LD chip with a wavelength of about 450nm, it emits high-brightness broadband yellow light at about 540nm. When the input power is 2.4W, 5wt% SrAl 2 O 4 -Ce:LuAG reaches a maximum luminous flux of 400lm.
[0042] Figure 1 The sample SrAl prepared in Example 2 of the present invention 2 O 4 -Ce:LuAG and LuAG, SrAl 2 O 4 XRD comparison diagram of Figure 1 It can be seen that 20wt% SrAl 2 O 4 -Ce:LuAG sample has diffraction peaks similar to SrAl 2 O 4 It corresponds well to the PDF card of the LuAG standard and no other impurities are produced, indicating that the crystallization performance of the sample is good.
[0043] Figure 2 The sample SrAl prepared in Example 2 of the present invention 2 O 4 -EL spectrum of Ce:LuAG under the excitation of 450nm LD chip; when the input power is 5W, its luminous flux reaches 1000lm.
[0044] Figure 3The samples SrAl prepared in Example 1 and Example 2 of the present invention 2 O 4 The relationship between the luminous flux of 25% and 20% of the total mass of ceramic raw materials and pure Ce:LuAG and the input power of the LD chip. Figure 3 It can be seen that compared with pure Ce:LuAG, it exhibits excellent luminescence performance under the excitation of blue light LD. When the input power is 5W, 20wt% SrAl 2 O 4 -Ce:LuAG has no luminous saturation and its maximum luminous flux can reach 1000lm.
[0045] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting, characterized in that: The composite fluorescent ceramic is prepared by spark plasma sintering using Ce:LuAG powder and SrAl2O4 powder as ceramic raw material powders, wherein Ce:LuAG is used as the ceramic main body and SrAl2O4 is introduced as the second phase. The prepared composite fluorescent ceramic has high brightness and high luminous efficiency. The method for preparing the composite fluorescent ceramic specifically comprises the following steps: S1: Weigh Ce:LuAG powder and SrAl2O4 powder according to the mass ratio respectively as ceramic raw material powders, wherein SrAl2O4 powder accounts for 5% to 25% of the total mass of the ceramic raw material powders; S2: Ce: LuAG powder and SrAl2O4 powder are blended and then anhydrous ethanol is added, and the mixture is fully mixed by ball milling; S3: taking out the slurry obtained after ball milling and drying it to obtain dry powder; S4: spark plasma sintering the dried powder under vacuum, and cooling to room temperature to obtain a composite fluorescent ceramic; In step S4, the sintering pressure of the spark plasma sintering is 50-100 MPa, the pulse current is 200-400 A, the heat preservation sintering time is 20-50 min, and the sintering temperature is 1650° C.-1800° C.
2. The high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S1, the particle size of the Ce:LuAG powder is 1 μm to 1.3 μm, the particle size of the SrAl2O4 powder is 1.5 μm to 2 μm, and the purity of both is above 99.99%.
3. The high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S2, the ball milling speed is 180-250 rpm, and the ball milling time is 15-30 h.
4. The high-brightness and high-luminous-efficiency composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S3, the drying temperature is 70-90° C. and the drying time is 8-12 hours.