A perfluoropolyether block polymer and its preparation method and application
The perfluoropolyether and polypolyol block polymer guided by isocyanate solve the problems of poor mechanical properties and irreversible driving caused by the crystalline properties of polymer materials, and achieve high toughness, tear resistance and high energy density Features, suitable for a variety of application fields.
Patent Information
- Application Number
- CN202310240859.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-13
AI Technical Summary
Existing polymer materials have problems such as poor mechanical properties, high Young's modulus, low energy density, irreversible drive and difficulty in recycling caused by crystallization characteristics, which limit their application in the medical, mechanical and electronic fields.
Isocyanate-guided perfluoropolyether and polypolyol form block polymers. Through the synergistic interaction between the perfluoropolyether segment and the polypolyol segment, a cluster structure is formed, which inhibits crystallinity and achieves reversible driving. and high energy density.
The material has high toughness, tear resistance, puncture resistance, recyclability and stimulation response characteristics, and has reduced Young's modulus and improved energy density. It is suitable for flexible electronic devices, artificial muscles and smart clothing.
Smart Images

Figure CN116425940B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new materials, and specifically relates to a perfluoropolyether block polymer material and a preparation method and application thereof. Background Art
[0002] Traditional crystalline polymer materials such as polyethylene glycol or polyethylene oxide (PEG or PEO), polylactic acid (PLLA), polycaprolactone (PCL), polytetramethylenetetramethylene glycol (PTMEG) have excellent comprehensive properties and are widely used in medical, mechanical, electrical, electronic, aerospace, new energy and other fields.
[0003] On the one hand, polymer crystallization gives this type of polymer material a high mechanical strength, but on the other hand, polymer crystallization also brings many disadvantages and shortcomings. Usually, this type of polymer material has high brittleness, insufficient toughness, and poor elasticity, which greatly limits its application. In order to improve the mechanical properties of this type of polymer material, previous studies have mainly focused on physical doping modification, by adding some physical fillers (such as carbon black, carbon nanotubes, polyethylene and other polymer materials) and chemical crosslinking (adding crosslinking agents to form a three-dimensional network) to improve the toughness and mechanical strength of the material, but physical doping is usually difficult to inhibit the crystallization of the material, and physical doping is difficult to make the filler uniformly dispersed in the substrate, requiring huge energy consumption. Thermosetting materials formed by chemical crosslinking can inhibit crystallization to a certain extent, but it is still difficult to obtain materials with high toughness and elasticity. In addition, physically doped and chemically crosslinked polymers are difficult to recycle for secondary use, which puts great pressure on the environment.
[0004] Artificial muscles based on shape memory materials have great application prospects in the field of flexible and miniaturized robots, but the existing materials have disadvantages such as low energy density, short driving distance, complex preparation process, and excessive Young's modulus, which leads to the fact that most artificial muscles based on shape memory cannot match the human body mechanics well. This is mainly related to the crystallization characteristics of the shape memory material itself. How to make artificial muscles have a lower Young's modulus and excellent driving performance at the same time has not been reported yet. Shape memory materials mainly include shape memory alloys and shape memory polymers. In contrast, shape memory polymers have received widespread attention in recent years due to their excellent performance. Among them, polycaprolactone is a typical representative, but its disadvantages are also very obvious, with high Young's modulus, poor mechanical matching, and inability to be reversibly driven.
[0005] Artificial tendons and artificial blood vessels have been widely used in the medical field. Although many of them have been industrialized and successfully applied to the human body, there are still many defects and shortcomings, such as poor permeability, mechanical properties that cannot match tissues, and non-degradability. Polylactic acid and polycaprolactone have good biocompatibility and are easy to degrade, but their disadvantages of easy crystallization and high modulus are also obvious.
[0006] Dielectric actuators have received extensive attention and applications in the fields of flexible tactile actuators, flexible robot actuators, small aircraft, and deep-sea robots. Existing dielectric elastomers are mainly 3MVHB and PDMS, both of which have excellent dielectric and mechanical properties. 3MVHB and silicone elastomers have high dielectric constants and therefore high energy density, but their viscosity (signal delay) and poor mechanical properties hinder their application in tactile actuators. Although silicone elastomers have good elasticity, their dielectric constants are small, and they usually require ultra-high driving voltages (>5kV) and pre-stretching to obtain better driving performance. These two obvious disadvantages greatly limit their industrial applications.
[0007] Perfluoropolyether is a type of fluorinated polymer with -OCF2-, -OCF2CF2-, and -OCF2CF(CF3)- as basic repeating units. Its unique ether oxygen structure also gives it physical and chemical properties that are different from traditional fluorinated polymers (such as polytetrafluoroethylene). On the one hand, the weak intermolecular interaction between perfluoropolyether segments and the high fluidity of the segments give it excellent tribological properties, making it widely used in lubricants. However, it also makes it difficult for perfluoropolyether polymers to form films and have poor mechanical properties, making it difficult to fully utilize the excellent properties of perfluoropolyether in the field of polymer materials. Summary of the invention
[0008] In view of the problems of polymer crystallization, large Young's modulus, poor comprehensive mechanical properties, small dielectric constant, poor film-forming property and single function in the above-mentioned prior art, the present invention provides a perfluoropolyether block polymer and its preparation method and application. The material is a block polymer formed by isocyanate-guided perfluoropolyether and polyol, and the perfluoropolyether chain blocks are evenly distributed on the polymer main chain, which effectively avoids the phase separation caused by physical blending and more effectively interacts with the polyol chain segments, so that the material has high toughness, tear resistance, puncture resistance, high dielectric constant, recyclability and stimulus response characteristics.
[0009] To achieve the above object, the present invention adopts the following technical solution:
[0010] A perfluoropolyether block polymer, the structural formula is:
[0011]
[0012] in, is a perfluoropolyether segment, 0≤x≤20, 0≤y≤50, 0≤z≤50, 0≤q≤20, and x, y, z and q are not 0 at the same time; wherein R1 is a spacer group of two -NCO in isocyanate, and R2 is a spacer group of -OH in organic polyol polymer. The differences among x, y, z and q represent different segment lengths of perfluoropolyether.
[0013] The sizes of x, y, z and q vary according to the molecular weight of the perfluoropolyether chain segment and can be integers or decimals.
[0014] Preferably, R1 is:
[0015] -(CH2)6-,
[0016] Preferably, R2 is:
[0017] Wherein, n is an integer.
[0018] More preferably, R2 is:
[0019]
[0020] The present invention further provides a method for preparing the above-mentioned perfluoropolyether block polymer, comprising the following steps:
[0021] (1) Under anhydrous and oxygen-free conditions, a hydroxyl-terminated perfluoropolyether oligomer, an isocyanate and a catalyst are reacted in an ultra-dry organic solvent at 60 to 85° C. to obtain an isocyanate-terminated perfluoropolyether;
[0022] (2) adding an organic solution of an organic polyol polymer to the isocyanate-terminated perfluoropolyether obtained in step (1), and reacting at 60 to 85° C. to obtain;
[0023] Wherein, the ratio of the total molar number of hydroxyl groups of the terminal hydroxyl perfluoropolyether oligomer and the organic polyol polymer to the molar number of isocyanate groups of the isocyanate is 1:1 to 1:1.2.
[0024] Preferably, the molar ratio of the perfluoropolyether oligomer to the organic polyol polymer is 2:1 to 1:8.
[0025] Preferably, the molecular weight of the hydroxyl-terminated perfluoropolyether oligomer is 500 to 5000, more preferably 1000 to 3000, such as E10H or D10H.
[0026] Preferably, the relative molecular mass of the organic polyol polymer is 500-10000, more preferably 500-3000.
[0027] Preferably, the organic polyol polymer is polycaprolactone diol, polyethylene glycol, polyether diol, polylactide diol or polypropylene glycol. More preferably, the organic polyol polymer is polycaprolactone diol, polypropylene glycol or polylactide diol.
[0028] Preferably, the catalyst in step (1) is an organic metal catalyst or a tertiary amine catalyst.
[0029] Preferably, the reaction time in step (1) is 40 to 80 minutes.
[0030] Preferably, the organometallic catalyst is an organotin catalyst, an organozinc catalyst or an organobismuth catalyst.
[0031] Preferably, the tertiary amine catalyst is triethylamine or diethylenetriamine.
[0032] Preferably, the ultra-dry organic solvent described in step (1) or the solvent of the organic solution of the organic polyol polymer described in step (2) is one or more of benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran or acetonitrile.
[0033] The present invention also provides applications of the above-mentioned perfluoropolyether block polymer, which includes: preparing flexible electronic devices, flexible actuators, artificial muscles, artificial tendons, artificial blood vessels, smart clothing or protective equipment.
[0034] Preferably, in the application of the perfluoropolyether block polymer in preparing artificial muscles, smart clothing or protective equipment, the structure of R2 is One or two of the above, with a molecular weight of 1500 to 10000.
[0035] Preferably, in the application of the perfluoropolyether block polymer in preparing flexible electronic devices, flexible actuators, artificial tendons, and artificial blood vessels, the structure of R2 is One or more of the above, with a molecular weight of 500 to 3000.
[0036] When the perfluoropolyether block polymer with the above specific structure is used in the above specific fields, it can obtain better performance than other perfluoropolyether block polymers.
[0037] The beneficial effects of the present invention are:
[0038] (1) The present invention forms a perfluoropolyether in an organic polyol polymer segment. Compared with the stable and large crystals formed between the highly regular organic polyol polymer segments, the mismatch between the perfluoropolyether and organic polyol polymer structures and the large van der Waals radius of the CF2 group destroy the regularity of the polyester block, thereby inhibiting the crystallinity of the material. The cluster structure is formed through dipole-dipole interaction and hydrogen bond interaction. The introduction of the perfluoropolyether segment greatly increases the solid-state entropy of the material, effectively balancing the temperature-induced crystallization and the strain-induced crystallization. When not stretched, the material tends to The organic polyol polymer is in an amorphous state, which greatly reduces the Young's modulus (3-5MPa) of the organic polyol polymer, which is equivalent to the Young's modulus of human tissue (<10MPa), showing excellent flexibility, soft and tough, and does not crystallize at room temperature; when subjected to external force, the polymer chain re-orients and strain-induced crystallization occurs. The stress of the material increases rapidly with the increase of strain, which enables the material to obtain ultra-high mechanical strength comparable to spider silk and excellent tear resistance. At the same time, due to the excellent tribological properties of perfluoropolyether, high-density chain segments can easily slip, so that the material has high ductility, high toughness and puncture resistance. The reversible physical crosslinking and slippage between molecular chains formed between perfluoropolyether segments and organic polyol polymer segments effectively improve the one-way irreversible shape memory properties of traditional organic polyol polymers. Under thermal stimulation, the new material can be reversibly reciprocated and has a high energy density (1450Jkg -1 ), far exceeding the 39Jkg of mammalian muscle -1 Since the material is in-situ cross-linked through physical interactions, it can be easily recycled under mild conditions and can still maintain more than 90% of its initial mechanical strength after more than three recycling cycles.
[0039] The present invention improves the deficiencies of organic polyol polymers by strategically utilizing the physicochemical properties of perfluoropolyethers and effectively combines the advantages of the two, so that the material has excellent performance that exceeds the existing technology, and has high toughness, tear resistance, puncture resistance, recyclability and stimulus response characteristics.
[0040] Compared with existing stimulus-responsive materials, the material of the present invention has the following advantages: compared with soft actuators such as liquid crystal elastomers and dielectric elastomers, the material of the present invention has higher energy density and equivalent Young's modulus, and at the same time has higher mechanical strength, tear resistance, and the ability to resist external damage; compared with traditional shape memory actuators, this material has a lower Young's modulus, higher energy density, a larger driving distance, and a simpler preparation method, and also realizes reversible driving, which is not available in previous shape memory actuators.
[0041] The material of the present invention has training enhancement properties similar to muscles. Through repeated mechanical training, the mechanical strength of the material can be effectively controlled, and after training, the mechanical properties are further enhanced. Compared with physical doping or chemical modification, the material of the present invention can be freely switched between different strengths and strength can be controlled according to different application scenarios, which is simple and effective.
[0042] The material of the present invention has a toughness that exceeds that of spider silk and Kevlar, and has a lower Young's modulus. Compared with natural spider silk, the material of the present invention completely replicates all the functions of spider silk, including ultra-high toughness, switchable strength, stimulus response, and can be recycled under mild conditions.
[0043] The material of the present invention exhibits different properties from traditional puncture-resistant materials. Compared with the prior art, the material of the present invention has the highest puncture resistance and can recover to its original state through shape memory after being damaged. It can still maintain its mechanical properties after repeated puncture for more than 3 times.
[0044] (2) In the application field of flexible actuators, the tactile actuator needs to have a modulus that matches the human body mechanics to ensure comfort, high elasticity to ensure that the driving signal has no hysteresis, and a high dielectric constant to ensure that it can be driven at low voltage while having high energy density. However, due to the strong interaction between chain segments, single polyether and polyester polymers usually have a high Young's modulus and poor elasticity, which makes it difficult to match the mechanics of the human body. Perfluoropolyether polymers are in a viscous flow state due to their weak interaction between chain segments, high flexibility and difficulty in crystallization, making them difficult to form films. The present invention successfully transforms the mechanical disadvantages of the two materials into advantages by combining the two materials, and obtains new performance to meet the performance requirements of the tactile actuator.
[0045] The material of the present invention has a high dielectric constant, so that the material can be driven at a low voltage; low dielectric loss, low viscoelasticity, and strain enhancement performance, so that it has the characteristics of high energy density, rapid response, and high electrochemical stability.
[0046] Compared with common dielectric elastomers such as 3MVHB and silicone elastomers, the material of the present invention has a higher dielectric constant and better mechanical properties, ensuring that the material can respond quickly under low voltage drive.
[0047] The material of the present invention has good hydrophilicity, which ensures that it can interact well with the electrode material when coating the electrode, so that the electrode material can stably adhere to the surface of the material, and when spraying the electrode, the electrode material can be well spread to obtain a uniform electrode that is not easy to fall off.
[0048] The material of the present invention has a self-repairing property under the assistance of heating. When preparing a laminated device, the laminated structure can be easily obtained by dry hot pressing, thus avoiding cumbersome processes and facilitating large-scale preparation.
[0049] The material of the present invention has a driving voltage much lower than that of the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is the infrared characterization spectrum of the specimens prepared in Examples 1 to 6 in Example 15.
[0051] Figure 2 This is the DSC characterization spectrum of the specimens prepared in Examples 1 to 6 in Example 15.
[0052] Figure 3 This is the XRD characterization spectrum of the specimens prepared in Examples 1 to 6 in Example 15.
[0053] Figure 4 This is a characterization graph of the stress-strain test of the specimens prepared in Examples 1 to 6 in Example 15.
[0054] Figure 5 This is the tear resistance characterization spectrum of the sample prepared in Example 3 in Example 15.
[0055] Figure 6 This is the puncture resistance characterization spectrum of the sample prepared in Example 3 in Example 15.
[0056] Figure 7 This is the shape memory test spectrum of the sample prepared in Example 3 in Example 15.
[0057] Figure 8 This is a characterization graph of the stress-strain test of the specimens prepared in Examples 7 to 9 in Example 15.
[0058] Fig. 9 This is the infrared characterization spectrum of the specimens prepared in Examples 7 to 9 in Example 15.
[0059] Fig.10 This is the XRD characterization spectrum of the specimens prepared in Examples 7 to 9 in Example 15.
[0060] Fig.11 This is a characterization graph of the stress-strain test of the specimens prepared in Examples 10 to 12 in Example 15.
[0061] Fig.12 This is a characterization diagram of the cyclic stress-strain test of the specimen prepared in Example 10 in Example 15.
[0062] Fig.13This is a characterization graph of the stress-strain test of the specimens prepared in Example 10 and commercial dielectric materials in Example 15.
[0063] Fig.14 This is the DSC characteristic spectrum of the specimens prepared in Examples 10 to 12 in Example 15.
[0064] Fig.15 This is the infrared characterization spectrum of the specimens prepared in Examples 10 to 12 in Example 15.
[0065] Fig.16 This is the dielectric test spectrum of the specimens prepared in Example 10 and commercial dielectric materials in Example 15.
[0066] Fig.17 This is a characterization graph of the stress-strain test of the specimens prepared in Examples 13 to 14 in Example 15. DETAILED DESCRIPTION
[0067] Example 1
[0068] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0069] 2 g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:1, and the ratio of the total hydroxyl number to isocyanate was 1:1.
[0070] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0071] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE1-PCL1.
[0072] By cutting the material into samples of appropriate size and repeatedly stretching it under different strains and training times, the mechanical strength of the material can be rapidly enhanced while also having stimulus-responsive properties.
[0073] Example 2
[0074] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 0.72g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0075] 1.6 g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:2, and the ratio of the total hydroxyl number to isocyanate was 1:1.05.
[0076] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0077] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE1-PCL2.
[0078] By cutting the material into samples of appropriate size and repeatedly stretching it under different strains and training times, the mechanical strength of the material can be rapidly enhanced while also having stimulus-responsive properties.
[0079] Example 3
[0080] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 0.5g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added into the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0081] 1.5 g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:3, and the ratio of the total hydroxyl number to isocyanate was 1:1.2.
[0082] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0083] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE1-PCL3.
[0084] By cutting the material into samples of appropriate size and repeatedly stretching it under different strains and training times, the mechanical strength of the material can be rapidly enhanced while also having stimulus-responsive properties.
[0085] Example 4 (Comparative Example)
[0086] Prepare samples with too high perfluoropolyether content for comparison:
[0087] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.44g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0088] 0.8 g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:3, and the ratio of the total hydroxyl number to isocyanate was 1:1.05.
[0089] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0090] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE2-PCL1.
[0091] Example 5
[0092] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 0.36g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0093] 2.0 g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5 mL of N,N-dimethylacetamide, and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:5, and the ratio of the total hydroxyl number to isocyanate was 1:1.0.5.
[0094] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0095] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE1-PCL5.
[0096] By cutting the material into samples of appropriate size and repeatedly stretching it under different strains and training times, the mechanical strength of the material can be rapidly enhanced while also having stimulus-responsive properties.
[0097] Example 6 (Comparative Example)
[0098] A sample without perfluoropolyether block was prepared as a comparison:
[0099] A 100mL two-necked flask was connected to a double-row tube, and the mixture was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes. Then, 2.0g of polycaprolactone diol with a relative molecular mass of 2000 was dissolved in 5mL of ultra-dry N,N-dimethylacetamide, 0.0.18g of 1,6-hexanediisocyanate and 0.01g of dibutyltin dilaurate were dissolved in 3mL of ultra-dry xylene, and added to the flask through syringes respectively. The reaction temperature was controlled to be 85°C and the stirring speed was 200r / min. The reaction temperature was maintained at 85°C and the stirring speed was 300r / min. The ratio of the total hydroxyl number to the isocyanate group was 1:1.0.5. The change in the viscosity of the system was observed. After the viscosity increased, ultra-dry N,N-dimethylacetamide was added to the system in small amounts and multiple times, 3 to 5mL each time, to ensure that the system had a viscosity that could be normally stirred at 50 to 100r / min. The reaction lasted for 10 to 15h.
[0100] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain polycaprolactone without perfluoropolyether, which is marked as PFPE0-PCL1.
[0101] Example 7
[0102] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0103] 3 g of polycaprolactone diol with a relative molecular mass of 3000 was dissolved in 5 mL of N,N-dimethylacetamide, and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The molar ratio of perfluoropolyether to polycaprolactone diol was 1:1, and the ratio of the total hydroxyl number to isocyanate was 1:1.
[0104] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.
[0105] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is marked as PFPE-PCL3000-1-1.
[0106] Example 8
[0107] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 0.72g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0108] Dissolve 2.4g of polycaprolactone diol with a relative molecular mass of 3000 in 5mL N,N-dimethylacetamide, and then add it to the above system with a syringe, keep the reaction temperature at 85℃, stir at 300r / min, the molar ratio of perfluoropolyether and polycaprolactone diol is 1:1, and the ratio of total hydroxyl number and isocyanate is 1:1.05. Observe the change of the viscosity of the system. After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3-5mL each time, to ensure that the system can be stirred normally at 50-100r / min. The reaction lasts for 10-15h.
[0109] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is marked as PFPE-PCL3000-1-2.
[0110] Example 9
[0111] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 0.5g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added into the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0112] 2.25 g of polycaprolactone diol with a relative molecular mass of 3000 was dissolved in 5 mL of N, N-dimethylacetamide, and then added to the above system with a syringe, the reaction temperature was maintained at 85°C, the stirring speed was 300 r / min, the molar ratio of perfluoropolyether and polycaprolactone diol was 1:1, and the ratio of total hydroxyl number to isocyanate was 1:1.05. The change in the viscosity of the system was observed. After the viscosity increased, ultra-dry N, N-dimethylacetamide was added to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system had a viscosity that could be normally stirred at 50 to 100 r / min. The reaction lasted for 10 to 15 hours.
[0113] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE-PCL3000-1-3.
[0114] Example 10
[0115] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.21g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0116] 1 g of polycaprolactone diol with a relative molecular mass of 1000 was dissolved in 5 mL of N, N-dimethylacetamide, and then added to the above system with a syringe, the reaction temperature was maintained at 85°C, the stirring speed was 300 r / min, the molar ratio of perfluoropolyether and polycaprolactone diol was 1:1, and the ratio of total hydroxyl number to isocyanate was 1:1.05. The change in the viscosity of the system was observed. After the viscosity increased, ultra-dry N, N-dimethylacetamide was added to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system had a viscosity that could be normally stirred at 50 to 100 r / min, and the reaction lasted for 10 to 15 hours.
[0117] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is marked as PFPE-PCL1000-1-1.
[0118] Weigh 1.2 g of the obtained material, dissolve it in 6 mL of N,N-dimethylacetamide solution, pour it into a polypropylene mold, put it into a vacuum dryer and degas for 10 minutes under vacuum, then take it out and place it on an absolute water platform to dry at room temperature for 3 to 5 days, and then put it in a 70°C oven to dry for 24 hours.
[0119] The obtained film was cut into strips of 1.5×1.5 cm in size, and then its surface was covered with a mask of 1×1 cm square size. After single-walled carbon nanotube electrodes were sprayed on both sides, the desired actuator was obtained.
[0120] Embodiment 11
[0121] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.44g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0122] 1.6 g of polycaprolactone diol with a relative molecular mass of 1000 was dissolved in 5 mL of N, N-dimethylacetamide, and then added to the above system with a syringe, the reaction temperature was maintained at 85°C, the stirring speed was 300 r / min, the molar ratio of perfluoropolyether to polycaprolactone diol was 1:2, the total hydroxyl number and isocyanate ratio was 1:1.05, and the change in the viscosity of the system was observed. After the viscosity increased, ultra-dry N, N-dimethylacetamide was added to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system had a viscosity that could be normally stirred at 50 to 100 r / min, and the reaction lasted for 10 to 15 hours.
[0123] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE-PCL1000-1-2.
[0124] Example 12
[0125] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.0g of a perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0126] 1.5 g of polyethylene glycol with a relative molecular mass of 1000 was dissolved in 5 mL of N, N-dimethylacetamide, and then added to the above system with a syringe, the reaction temperature was maintained at 85°C, the stirring speed was 300 r / min, the molar ratio of perfluoropolyether and polycaprolactone diol was 1:3, the ratio of total hydroxyl number and isocyanate was 1:1.05, and the change in the viscosity of the system was observed. After the viscosity increased, ultra-dry N, N-dimethylacetamide was added to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system had a viscosity that could be normally stirred at 50 to 100 r / min, and the reaction lasted for 10 to 15 hours.
[0127] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE-PCL1000-1-3.
[0128] Example 13
[0129] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 2g of a perfluoropolyether oligomer with a relative molecular weight of about 500, 2.5g of dicyclohexylmethylene diisocyanate, 0.01g of an organic bismuth composite catalyst (BiCAT), and ultra-dry toluene were added to the flask through a syringe, the reaction temperature was controlled to 60°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0130] 4 g of polylactide diol with a relative molecular mass of 1000 was dissolved in N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 60°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The total hydroxyl number and isocyanate ratio of perfluoropolyether and polylactide diol was 1:1.2.
[0131] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times to ensure that the system has a viscosity that allows normal stirring at 50-100 r / min. The reaction lasts for 10-15 hours.
[0132] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is labeled as PFPE-PLLA.
[0133] Embodiment 14
[0134] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 2g of a perfluoropolyether oligomer with a relative molecular weight of about 1000, 1.2g of 4,4'-diphenylmethane diisocyanate, triethylamine, and ultra-dry toluene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.
[0135] 3 g of polypropylene glycol with a relative molecular mass of 3000 was dissolved in tetrahydrofuran and then added into the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The change in the viscosity of the system was observed. The total hydroxyl number and isocyanate ratio of perfluoropolyether and polypropylene glycol was 1:1.2.
[0136] After the viscosity increases, add ultra-dry tetrahydrofuran to the system in small amounts and multiple times to ensure that the system has a viscosity that allows normal stirring at 50-100 r / min. The reaction continues for 10-15 hours.
[0137] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 3 to 5 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain a perfluoropolyether block polymer, which is marked as PFPE-PPG.
[0138] Embodiment 15
[0139] The samples obtained in Examples 1 to 6 were subjected to infrared testing and the results obtained were as follows: Figure 1 As shown in the figure, the perfluoropolyether block polymer was successfully synthesized, and hydrogen bonding and dipole-dipole interaction were formed between the perfluoropolyether segments and the polycaprolactone segments. Moreover, the introduction of perfluoropolyether successfully inhibited the crystallization of polycaprolactone diol.
[0140] The samples obtained in Examples 1 to 6 were subjected to DSC and XRD tests. The results obtained are as follows: Figure 2 and Figure 3 The results further show that the introduction of perfluoropolyether can effectively inhibit the crystallization of polycaprolactone.
[0141] The specimens obtained in Examples 1 to 6 were tested by a universal tensile machine and the results obtained were as follows: Figure 4 As shown in the figure, when the ratio of perfluoropolyether to polycaprolactone is 1:3 to 1:1 (PFPE1-PCL3, PFPE1-PCL2, PFPE1-PCL1), the material can take into account low Young's modulus (3 to 5MPa), high elongation (2100% to 2300%), high tensile strength (50 to 73MPa) and high toughness (741MJm -3 ), when the content of perfluoropolyether is too high (PFPE2-PCL1), the mechanical strength of the material decreases rapidly, and when the content of polycaprolactone is too high, the Young's modulus will be too high, and the toughness and flexibility will be lost. Compared with the existing technology (Adv. Mater. 2020, 32, 2005759., Adv. Mater. 2021, 33, 2105829., Adv. Mater. 2021, 33, 2101498.), the material of the present invention shows great superiority, having the highest toughness while having a lower Young's modulus in the existing reported technology.
[0142] The strips obtained in Example 3 were subjected to tear resistance test and the results were as follows: Figure 5 Compared with the prior art (Adv. Mater. 2020, 32, 2005759., Adv. Mater. 2021, 33, 2101498. Mater. Horizons 2021, 8, 2742.), the material of the present invention has the highest tear resistance (712.3 MJm -2 ).
[0143] The samples obtained in Example 3 were subjected to puncture resistance test, and the results obtained were as follows: Figure 6 It can be seen that the material of the present invention has excellent puncture resistance and can achieve repeated puncture resistance through shape memory.
[0144] The shape memory test was performed on the sample obtained in Example 3. The results are as follows: Figure 7 It can be seen that the material of the present invention has stimulus response characteristics.
[0145] The above results show that by strategically utilizing the physicochemical properties of perfluoropolyether to improve the shortcomings of organic polyol polymers and effectively combining the advantages of the two, the material has excellent performance that exceeds the existing technology, and has high toughness, tear resistance, puncture resistance, recyclability and stimulus response characteristics, which are not available in the existing technology.
[0146] The specimens obtained in Examples 7 to 9 were tested by a universal tensile machine. The results obtained are as follows: Figure 8Perfluoropolyether effectively improves the mechanical properties of high molecular weight organic polyols, ensuring that the material has high mechanical strength while having a low Young's modulus.
[0147] The samples obtained in Examples 7 to 9 were subjected to infrared and XRD tests. The results obtained are as follows: Fig. 9 and Fig.10 The introduction of perfluoropolyether effectively inhibits the crystallization of high molecular weight organic polyols.
[0148] The specimens obtained in Examples 10 to 12 were tested by a universal tensile machine and the results obtained were as follows: Figures 11 to 13 The obtained spline has a very low Young's modulus, flexibility and excellent elasticity, which is comparable to the mechanical properties of existing commercial dielectric materials ( Fig.13 Compared with 3M, Dragonskin, PDMS and Ecoflex), the material of the present invention has more excellent mechanical properties.
[0149] The samples obtained in Examples 10 to 12 were subjected to DSC and infrared tests. The results obtained are as follows: Fig.14 and 15 As shown in the figure, the material is amorphous, and the introduction of perfluoropolyether effectively improves the crystallization problem of organic polyols.
[0150] The test strips obtained in Example 10 and the commercial dielectric elastomer were subjected to dielectric testing and the results obtained were as follows: Fig.16 As shown. The introduction of perfluoropolyether improves the mechanical properties of organic polyols while enabling the material to obtain a high dielectric constant, which far exceeds the existing commercial dielectric materials ( Fig.16 3MVHB, Dragonskin, PDMS and Ecoflex).
[0151] The specimens obtained in Examples 13 to 14 were tested by a universal tensile machine. The results obtained are as follows: Fig.17 Perfluoropolyether effectively improves the mechanical properties of polylactide and polypropylene glycol, and has low Young's modulus and high mechanical strength.
Claims
1. A perfluoropolyether block polymer, characterized in that: The structural formula is: ; in, is a perfluoropolyether segment, 0≤x≤20, 0≤y≤50, 0≤z≤50, 0≤q≤20, and y and z are not 0 at the same time; R1 is a spacer group of two -NCO in isocyanate, R2 is: A spacer group between two -OH groups in polycaprolactone diol, a spacer group between two -OH groups in polyethylene glycol, a spacer group between two -OH groups in polytetramethylene glycol, a spacer group between two -OH groups in polylactide diol, or a spacer group between two -OH groups in polypropylene glycol; The perfluoropolyether block polymer is prepared by the following method: (1) Under anhydrous and oxygen-free conditions, a hydroxyl-terminated perfluoropolyether oligomer, an isocyanate and a catalyst are reacted in an ultra-dry organic solvent at 60-85° C. to obtain an isocyanate-terminated perfluoropolyether; (2) adding an organic solution of an organic polyol polymer to the isocyanate-terminated perfluoropolyether obtained in step (1), and reacting at 60-85° C. to obtain; Wherein, the ratio of the total molar number of hydroxyl groups of the terminal hydroxyl perfluoropolyether oligomer and the organic polyol polymer to the molar number of isocyanate groups of the isocyanate is 1:1 to 1:1.
2.
2. The perfluoropolyether block polymer according to claim 1, characterized in that: R1 is: , , , , , , , , , , , , , , , , , , , , , , , , , , or .
3. The perfluoropolyether block polymer according to claim 1, characterized in that: The molar ratio of the perfluoropolyether oligomer to the organic polyol polymer is 1:
1.
4. The perfluoropolyether block polymer according to claim 1, characterized in that: The molecular weight of the terminal hydroxyl perfluoropolyether oligomer is 500-5000; the relative molecular weight of the organic polyol polymer is 500-10000.
5. The perfluoropolyether block polymer according to claim 4, characterized in that: The molecular weight of the terminal hydroxyl perfluoropolyether oligomer is 1000-3000; the relative molecular weight of the organic polyol polymer is 500-3000.
6. The perfluoropolyether block polymer according to claim 1, characterized in that: The catalyst in step (1) is an organic metal catalyst or a tertiary amine catalyst.
7. The perfluoropolyether block polymer according to claim 6, characterized in that: The organic metal catalyst is an organic tin catalyst, an organic zinc catalyst or an organic bismuth catalyst; the tertiary amine catalyst is triethylamine or diethylenetriamine.
8. The perfluoropolyether block polymer according to claim 1, characterized in that: The solvent of the organic solution of the organic polyol polymer in step (2) is one or more of benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran or acetonitrile.
9. The use of the perfluoropolyether block polymer according to claim 1, characterized in that: The applications include preparing flexible electronic devices, flexible actuators, artificial muscles, artificial tendons, artificial blood vessels, smart clothing or protective equipment.
10. The use according to claim 9, characterized in that: In the application of the perfluoropolyether block polymer in the preparation of artificial muscles, smart clothing or protective equipment, the R2 is one or both of the spacer groups of two -OH in polycaprolactone diol or the spacer groups of two -OH in polypropylene glycol, and the molecular weight is 1500~10000; in the application of the perfluoropolyether block polymer in the preparation of flexible electronic devices, flexible actuators, artificial tendons and artificial blood vessels, the R2 is one or more of the spacer groups of two -OH in polycaprolactone diol, the spacer groups of two -OH in polypropylene glycol or the spacer groups of two -OH in polylactide diol, and the molecular weight is 500~3000.