Preparation method and coating of AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating

By preparing AlN/Si/SiN/AlSiN/AlN/Al multi-layer gradient structure coatings on magnesium alloys and performing crystal growth control processing, the problem of insufficient corrosion resistance caused by continuous interlayer growth of ceramic coatings was solved and achieved The high-efficiency anti-corrosion performance of magnesium alloy is improved and the corrosion resistance time is extended.

CN116426875BActive Publication Date: 2024-10-25SOUTHWEST UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310411961.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-25
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Ceramic coatings of magnesium, aluminum-based light metals and their alloys have insufficient corrosion resistance in corrosive media. This is mainly due to the high hardness and large internal stress of the ceramic coating, which results in poor bonding between the substrate and the coating. Moreover, under the physical vapor deposition method The continuous growth defects between the layers of ceramic coatings provide channels for corrosive media, limiting the anti-corrosion performance of gradient multi-layer coatings.

Method used

Using the preparation method of AlN/Si/SiN/AlSiN/AlN/Al multi-layer gradient structure coating, by sequentially depositing an Al layer, a first AlN layer, an AlSiN layer, a SiN layer, a Si layer and a second AlN layer on the substrate, And before depositing certain layers, crystal growth control processing, such as exposure processing or oxygen ion bombardment, is performed to avoid continuous columnar growth between layers and form a discontinuous growth structure.

Benefits of technology

Significantly reduces the corrosion current density of magnesium alloys, improves corrosion resistance, and extends the immersion time in 3.5wt% NaCl solution. The discontinuous growth of the coating can reduce the corrosion current density by 6 orders of magnitude and increase the corrosion resistance immersion time. To 360h, the anti-corrosion performance of the coating is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116426875B_ABST
    Figure CN116426875B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of surface anti-corrosion coatings, and specifically discloses a preparation method and coating of an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, including the steps of sequentially depositing an Al layer, an AlN layer, an AlSiN layer, a SiN layer, a Si layer and an AlN layer on the surface of a substrate, and also including the steps of respectively performing crystal growth regulation treatment before the step of depositing the AlN layer and / or the AlSiN layer. The preparation method and coating provided by the present invention form a dual-phase gradient multilayer structure coating of Al and Si elements, and the gradient effect of the elements can weaken the transmission power of the corrosion charge and improve the corrosion resistance of the coating. At the same time, the crystal growth regulation treatment is adopted to suppress the continuous columnar growth defects between the AlSiN / AlN / Al layers, and the discontinuous growth structure blocks the penetration path of the corrosion ions, thereby greatly improving the anti-corrosion performance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of surface anti-corrosion coatings, and in particular, relates to a preparation method of an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating and the coating. Background Art

[0002] Due to their excellent performance, magnesium, aluminum-based light metals and their alloys have been widely used in aerospace, automotive industry, biomedicine, electronic digital and other fields. However, their corrosion resistance is extremely poor, especially magnesium alloys. Rapid corrosion degradation seriously restricts their further application in industrial production. Therefore, how to improve the corrosion resistance of magnesium, aluminum-based light metals and their alloys has become a bottleneck problem that must be urgently solved for their widespread application and industrialization. So far, many studies have been devoted to improving the corrosion resistance of magnesium, aluminum-based light metals and their alloys. Such as purification, alloying, heat treatment and coating technologies, among which surface coating technology can effectively separate magnesium alloys from corrosive media, improve corrosion resistance, and extend the service life of the substrate. Due to its economy and effectiveness, surface coating technology is considered to be the most promising technical solution to improve the corrosion resistance of magnesium, aluminum-based light metals and their alloys.

[0003] At present, the coatings on magnesium, aluminum-based light metals and their alloys mainly include pure metal coatings, polymer coatings, inorganic compound coatings, ceramic coatings, etc. Among the numerous coating materials, ceramic coatings, such as AlN, SiN, etc., have good chemical inertness, stability, and excellent hardness, and the raw materials are readily available, cheap, and easy to prepare. Therefore, magnesium, aluminum-based light metals and their alloys protected by ceramic coatings often have strong controllability, wide selectivity, and simple operability, and are also currently very mainstream solutions. Despite this, the ceramic-based coatings deposited on the surface of magnesium, aluminum-based light metals and their alloys are not perfect, and there are corresponding defects, such as high hardness and large internal stress of the ceramic coatings, which result in poor bonding between the ceramic-based coatings deposited on the surface of magnesium, aluminum-based light metals and their alloys and the substrate. To address this problem, the current mainstream technical solution is to design gradient multilayer coatings.

[0004] However, due to the inherent growth characteristics of ceramic coatings, especially ceramic coatings prepared by physical vapor deposition methods, defects of continuous interlayer growth are prone to occur between coatings of the same element. This defect provides a corrosion channel for the corrosive medium, which greatly limits the anti-corrosion performance of the gradient multilayer coating. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating and the coating, wherein the method can improve the anti-corrosion performance of the gradient multilayer coating.

[0006] In a first aspect, the present invention provides a method for preparing an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, comprising the steps of sequentially depositing an Al layer, a first AlN layer, an AlSiN layer, a SiN layer, a Si layer and a second AlN layer on a substrate surface, and also comprising the step of performing a crystal growth regulation treatment before the step of depositing the AlN layer and / or the AlSiN layer;

[0007] The step of crystal growth regulation treatment before depositing the first AlN layer comprises at least one of exposing the Al layer deposited on the substrate in an oxygen-containing atmosphere or bombarding the Al layer with oxygen ions in an oxygen-containing atmosphere; and / or,

[0008] The step of crystal growth regulation treatment before depositing the AlSiN layer comprises at least one of exposing the AlN / Al layer deposited on the substrate in an oxygen-containing atmosphere or bombarding it with oxygen ions in an oxygen-containing atmosphere.

[0009] Optionally, the steps of depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer adopt at least one of vacuum evaporation, sputtering coating, arc plasma coating, ion coating and molecular beam epitaxy coating.

[0010] Optionally, the step of crystal growth regulation treatment before depositing the AlN layer comprises exposing the Al layer deposited on the substrate to an atmospheric atmosphere; and / or,

[0011] The step of crystal growth regulation treatment before depositing the AlSiN layer comprises exposing the AlN / Al layer deposited on the substrate to an atmospheric atmosphere.

[0012] Optionally, the steps of depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer are performed by magnetron sputtering coating.

[0013] Optionally, depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer comprises the following steps:

[0014] (1) placing the polished substrate in a sputtering chamber of a magnetron sputtering coating machine, evacuating the chamber, and then performing ion bombardment etching in an argon atmosphere;

[0015] (2) turning on a direct current power supply of an Al target in an argon atmosphere to deposit an Al layer on the surface of the substrate;

[0016] (3) subjecting the deposited Al layer to a crystal growth control treatment and exposing it to an atmospheric atmosphere for more than 5 minutes;

[0017] (4) turning on an Al target power supply in a mixed atmosphere of argon and nitrogen to deposit a first AlN layer on the surface of the Al layer;

[0018] (5) subjecting the deposited first AlN layer to a crystal growth control treatment and exposing it to an atmospheric atmosphere for more than 5 minutes;

[0019] (6) turning on the power supplies of the Al target and the Si target simultaneously in a mixed atmosphere of argon and nitrogen to deposit an AlSiN layer on the surface of the first AlN layer;

[0020] (7) turning on the Si target power supply in a mixed atmosphere of argon and nitrogen to deposit a SiN layer on the surface of the AlSiN layer;

[0021] (8) turning on the Si target power supply in an argon atmosphere to deposit a Si layer on the surface of the SiN layer;

[0022] (9) In a mixed atmosphere of argon and nitrogen, an Al target power supply is turned on to deposit a second AlN layer on the surface of the Si layer.

[0023] Optionally, after the crystal growth regulation treatment, the deposited AlN / Al layer includes crystal plane diffraction peaks of AlN (100), (101), (102) and (112); and / or,

[0024] After the crystal growth control treatment, the deposited AlSiN / AlN / Al layer includes AlN (100) and (110) crystal plane diffraction peaks.

[0025] Optionally, after the crystal growth regulation treatment, the average grain size of the AlN (101) crystal plane in the deposited AlN / Al layer is 14.6 nm; and / or,

[0026] After the crystal growth regulation treatment, the average grain size of the AlN (100) crystal plane in the deposited AlSiN / AlN / Al layer is 12.5 nm.

[0027] Optionally, the first AlN layer and the Al layer are discontinuously columnarly grown; and / or,

[0028] The AlSiN layer and the first AlN layer are grown in a discontinuous columnar manner.

[0029] In a second aspect, the present invention provides an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, which is obtained by the aforementioned method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating.

[0030] Optionally, the thickness of the Al layer is 0.3-1.5 μm, the thickness of the first AlN layer is 0.3-1.5 μm, the thickness of the AlSiN layer is 0.3-1.5 μm, the thickness of the SiN layer is 0.1-0.6 μm, the thickness of the Si layer is 0.1-0.6 μm, and the thickness of the second AlN layer is 0.1-0.6 μm.

[0031] Optionally, the corrosion potential of the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure in a 3.5wt% NaCl solution is -1.46 V, and the corrosion current density is 4.75×10 −10 A / cm 2 , the polarization resistance is 5.48×10 7 Ω / cm 2 The corrosion rate is 5.52×10 -6 mm / year.

[0032] In summary, the present invention has at least one of the following beneficial effects:

[0033] 1. The present invention provides a method for preparing an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, wherein an Al layer, a first AlN layer, an AlSiN layer, a SiN layer, a Si layer and a second AlN layer are sequentially deposited on a substrate, the Al element is reduced from the Al base layer upwards, and the Si element is gradually increased from the AlSiN layer to form a dual-phase gradient structure coating. The gradient multilayer structure coating can reduce the corrosion current density of a substrate (such as a magnesium alloy) by 4 orders of magnitude, and improve the corrosion resistance immersion (in a 3.5wt% NaCl solution) to 144h, thereby greatly improving the corrosion resistance of the substrate. However, when the corrosive medium penetrates the SiN layer, the corrosive medium penetrates to the bottom of the coating through the continuous columnar defects in the AlSiN / AlN / Al layer, which damages the anti-corrosion performance of the coating. By performing crystal growth control treatment on the first AlN layer and / or the AlSiN layer, the growth of the continuous columnar structure can be avoided, thereby further improving the anti-corrosion performance of the gradient coating, which can reduce the corrosion current density of the substrate (such as magnesium alloy) by 6 orders of magnitude and improve the corrosion resistance to immersion for 360 hours. So far, there has been no report on reducing the corrosion current density of the substrate by 6 orders of magnitude. Therefore, this AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating has extremely excellent anti-corrosion performance.

[0034] 2. The present invention provides a method for preparing an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, which adopts physical vapor deposition, has a simple process and strong controllability. The step of crystal growth regulation treatment only requires exposing the coating in an oxygen-containing atmosphere or bombarding it with oxygen ions in an oxygen-containing atmosphere, that is, isolating the connection between the layers, and each layer grows independently, thereby avoiding the growth of a continuous columnar structure. The suppression of coarse continuous columnar defects can effectively block the corrosion path, thereby improving the anti-corrosion performance of the gradient coating. In addition, since the continuous columnar structure between layers is suppressed, the continuous growth of the grain size of the coating is also suppressed, the grains become smaller, and the grain refinement effect makes the interior of the coating denser, which is also beneficial to suppressing the penetration of corrosive media and improving the anti-corrosion performance.

[0035] 3. The AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating provided by the present invention has uniform and dense film formation, strong bonding with the substrate, strong load resistance, and excellent corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic structural diagram of the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating of the present invention.

[0037] Figure 2 It is a process flow chart of the preparation method of the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating of the present invention.

[0038] Figure 3 These are FESEM and EDX images of the continuously grown and discontinuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coatings prepared in Example 1.

[0039] Figure 4 1 and 2 are XRD patterns of the AlN single layer, the continuously grown AlN / Al coating and the discontinuously grown AlN / Al coating prepared in Example 1.

[0040] Figure 5 1 and 2 are XRD diagrams of the AlSiN single layer, continuously grown and discontinuously grown AlSiN / AlN / Al multilayer coatings prepared in Example 1.

[0041] Figure 6 It is the electrochemical polarization curve diagram of the continuously grown and discontinuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating prepared in Example 1 in 3.5wt% NaCl solution.

[0042] Figure 7This is a comparison chart of the immersion corrosion time of the continuously grown and discontinuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coatings prepared in Example 1 in a 3.5wt% NaCl solution.

[0043] Description of reference numerals:

[0044] 1. magnesium alloy substrate, 2. Al layer, 3. first AlN layer, 4. AlSiN layer, 5. SiN layer, 6. Si layer, 7. second AlN layer. DETAILED DESCRIPTION

[0045] The present invention provides a preparation method and coating of an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0046] The preparation method provided by the present invention is referred to Figure 1 , an Al layer 2, a first AlN layer 3, an AlSiN layer 4, a SiN layer 5, a Si layer 6 and a second AlN layer 7 are sequentially deposited on a magnesium alloy substrate 1 by physical vapor deposition, and the prepared multilayer AlSi-based ceramic material can improve the corrosion resistance of the magnesium alloy substrate 1; the Al element is reduced from the Al base layer upward, and the Si element is gradually increased from the AlSiN layer to form a dual-phase gradient structure coating. This dual-phase element gradient structure design can effectively alleviate the element potential difference between the Al layer and the Si layer, which is conducive to weakening the corrosion charge transmission power, thereby improving the corrosion resistance of the coating; at the same time, the hardness increases from the Al layer to the Si layer, which can alleviate the hardness difference between the soft layer and the hard layer and improve the coating's load resistance. Specifically, the continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating can reduce the corrosion current density of the magnesium alloy substrate in a 3.5wt% NaCl solution by 4 orders of magnitude, and the corrosion resistance immersion is increased to more than 144h, greatly improving the corrosion resistance of the substrate.

[0047] During the research, the inventors found that the multilayer gradient structure coating prepared by physical vapor deposition method is prone to the defect of continuous columnar growth between the coatings of the same element, especially between the interfaces of AlSiN / AlN / Al layers. This defect provides a corrosion channel for the corrosive medium, which greatly limits the anti-corrosion performance of the gradient multilayer coating. After a long period of research, the inventors surprisingly found that, referring to Figure 2, through crystal growth regulation treatment, that is, before depositing the first AlN layer, the Al layer deposited on the magnesium alloy substrate is exposed to an oxygen-containing atmosphere or subjected to oxygen ion bombardment in an oxygen-containing atmosphere, at least one of which can isolate the connection between the first AlN layer and the Al layer, so that the first AlN layer and the Al layer grow independently, thereby avoiding continuous columnar growth between the first AlN layer and the Al layer; similarly, before depositing the AlSiN layer, the AlN / Al layer of the substrate is exposed to an oxygen-containing atmosphere or subjected to oxygen ion bombardment in an oxygen-containing atmosphere, at least one of which can isolate the connection between the AlSiN layer and the first AlN layer, so that the AlSiN layer and the first AlN layer grow independently, thereby avoiding continuous columnar growth between the AlSiN layer and the first AlN layer; the suppression of coarse continuous columnar defects can effectively block the corrosion path, thereby improving the corrosion resistance of the gradient coating. In addition, since the continuous columnar growth between layers is suppressed, that is, the continuous growth of the grain size of AlN and AlSiN is also suppressed, the AlN and AlSiN grains become smaller, and the grain refinement effect makes the interior of the coating more compact, which is also beneficial to inhibit the penetration of corrosive media and improve the corrosion resistance. Therefore, the non-continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating prepared by this method can greatly improve the corrosion resistance of magnesium alloys. Specifically, the non-continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating can reduce the corrosion current density of the magnesium alloy substrate in 3.5wt% NaCl solution by 6 orders of magnitude, and improve the corrosion resistance immersion to more than 360h. So far, there has been no report on a coating that reduces the corrosion current density of the magnesium alloy substrate by 6 orders of magnitude.

[0048] In an embodiment of the present invention, the material of the above-mentioned substrate is not particularly limited as long as it is a metal material. That is, the above-mentioned discontinuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating is suitable for various corrosion-resistant metal materials. As some specific examples, the material of the above-mentioned substrate can be magnesium, aluminum-based metals and their light alloys, such as magnesium alloys.

[0049] The deposition step of the coating of the present invention adopts physical vapor deposition, including at least one of vacuum evaporation, sputtering coating, arc plasma coating, ion coating and molecular beam epitaxy coating, preferably sputtering coating, more preferably magnetron sputtering coating.

[0050] In some embodiments of the present invention, a magnetron sputtering coating method is used to prepare an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, which specifically includes the following steps:

[0051] (1) Place the polished substrate in the sputtering chamber of the magnetron sputtering coating machine and wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, ion bombardment etching was performed in an argon atmosphere;

[0052] (2) Turn on the Al target DC power supply in an argon atmosphere to deposit an Al base layer on the substrate surface;

[0053] (3) subjecting the deposited Al base layer to crystal growth regulation treatment;

[0054] (4) Wait until the chamber pressure is reduced to less than 1×10 -6 Torr, the Al target power supply is turned on in a mixed atmosphere of argon and nitrogen to deposit an AlN transition layer (the first AlN layer) on the surface of the Al base layer;

[0055] (5) performing crystal growth control treatment on the deposited AlN transition layer;

[0056] (6) Wait until the chamber pressure is reduced to less than 1×10 -6 Torr, in a mixed atmosphere of argon and nitrogen, power supplies of the Al target and the Si target are simultaneously turned on to deposit an AlSiN transition layer on the surface of the AlN transition layer;

[0057] (7) Wait until the chamber pressure is reduced to less than 1×10 -6 Torr, turning on the Si target power supply in a mixed atmosphere of argon and nitrogen to deposit a SiN transition layer on the surface of the AlSiN transition layer;

[0058] (8) Wait until the chamber pressure is reduced to less than 1×10 -6 When 2000 Å / min, the Si target power supply is turned on in an argon atmosphere to deposit a Si transition layer on the surface of the SiN transition layer;

[0059] (9) Wait until the chamber pressure is reduced to less than 1×10 -6 When 3000 Å / min, the Al target power supply was turned on in a mixed atmosphere of argon and nitrogen to deposit an AlN top layer (the second AlN layer) on the surface of the Si transition layer.

[0060] In some embodiments of the present invention, the Al target is an Al single target with a purity of not less than 99.9%, the Si target is an Si single target with a purity of not less than 99.9%, the argon gas is an argon single gas with a purity of not less than 99.999%, and the nitrogen gas is a nitrogen single gas with a purity of not less than 99.999%. Optionally, the temperatures of steps (1)-(9) are each independently maintained at room temperature to 300°C.

[0061] In step (1), the substrate is placed in a magnetron sputtering coating machine for argon ion bombardment and etching to remove the residual oxide layer or other impurities in the substrate, thereby ensuring that the coating has good bonding strength with the substrate.

[0062] In some embodiments of the present invention, the specific process and specific parameters in step (1) are not particularly limited as long as the above-mentioned purpose can be achieved. As a specific example, the substrate is placed on a turntable and sent into a sputtering chamber. The turntable speed is 30 r / min, the deposition chamber temperature is 25-300°C, and the vacuum is evacuated to less than 1×10 -6 After 3000 rpm, inert gas was introduced with a gas flow rate of 40-50 SCCM and a substrate negative bias voltage of 100-150 W, and ion bombardment was performed for 10-20 min.

[0063] In some embodiments of the present invention, the substrate needs to be pre-treated by grinding and polishing before being placed in the magnetron sputtering coating machine to provide a flat and smooth adhesion surface for subsequent coating. Furthermore, the specific process of pre-treatment is: the metal substrate is subjected to rough grinding, fine grinding, rough polishing, and fine polishing until it is a mirror surface without fine scratches, and ultrasonic cleaning is performed with acetone and anhydrous ethanol for 5-10 minutes in sequence.

[0064] In some embodiments of the present invention, in step (2), the flow rate of the argon atmosphere is 40-50 SCCM, the DC power is 300-400 W, the substrate negative bias voltage is 0-50 V, the turntable speed is 30 r / min, and the deposition pressure is 3.0-4.0×10 -3 Torr, the deposition rate is 15-20nm / min, and by controlling the deposition time, an Al base layer with a thickness of 0.3-1.5μm can be deposited.

[0065] In step (3), a new growth surface and nucleation site are provided for the growth of the next transition layer, the AlN layer, through the crystal growth regulation treatment, so that the continuous growth between the Al layer and the AlN layer can be suppressed, and the continuous columnar growth defects can be suppressed.

[0066] In the embodiment of the present invention, the specific process and specific parameters of step (3) are not particularly limited, and the sputtering chamber may be placed in an oxygen-containing atmosphere as a type of oxygen-containing atmosphere, or may be placed in an atmospheric atmosphere, as long as the above-mentioned purpose can be achieved. As a specific example, after depositing an Al base layer on the substrate, the substrate is placed in a transition chamber, and the transition chamber is ventilated with an atmospheric pressure of 1.0×10 -1Torr to atmospheric pressure level, the sample is exposed for more than 5 minutes, and then the exposed sample is placed in the sputtering chamber to prepare for the deposition of the next layer. As another specific example, the crystal growth regulation treatment can also be accelerated by directly introducing oxygen into the sputtering chamber, or bombarding the sample surface with oxygen ions in an oxygen atmosphere.

[0067] In some embodiments of the present invention, in step (4), the flow rate of the argon atmosphere is 40-50 SCCM, the flow rate of the nitrogen atmosphere is 9-12 SCCM, the DC power is 300-400 W, the turntable speed is 30 r / min, the substrate negative bias voltage is 0-50 V, and the deposition pressure is 3.0-4.0×10 -3 Torr, the deposition rate is 7-10nm / min. By controlling the deposition time, an AlN transition layer with a thickness of 0.3-1.5μm can be deposited.

[0068] In step (5), after the crystal growth regulation treatment, a new growth surface and nucleation site are provided for the growth of the next transition layer AlSiN, thereby suppressing the continuous growth between the AlN and AlSiN layers and suppressing the continuous columnar growth defects.

[0069] In the embodiment of the present invention, the specific process and specific parameters of this step are not particularly limited, and the sputtering process can be carried out in an oxygen-containing atmosphere in a sputtering chamber or in an atmospheric atmosphere, as long as the above-mentioned purpose can be achieved. As a specific example, after depositing an AlN transition layer on a substrate, the substrate is placed in a transition chamber, and the transition chamber is ventilated with an atmospheric pressure of 1.0×10 -1 Torr to atmospheric pressure level, the sample is exposed for more than 5 minutes, and then the exposed sample is placed in the sputtering chamber to prepare for the deposition of the next layer. As another specific example, the crystal growth regulation treatment can also be accelerated by directly introducing oxygen into the sputtering chamber, or bombarding the sample surface with oxygen ions in an oxygen atmosphere.

[0070] In some embodiments of the present invention, in step (6), the flow rate of the argon atmosphere is 40-50 SCCM, the flow rate of the nitrogen atmosphere is 9-12 SCCM, the DC power of the Al target is 300-400 W, the DC power of the Si target is 100-200 W, the negative bias voltage of the substrate is 0-50 V, the rotation speed of the turntable is 30 r / min, and the deposition pressure is 3.0-4.0×10 -3 Torr, the deposition rate is 10-15nm / min. By controlling the deposition time, an AlSiN transition layer with a thickness of 0.3-1.5μm can be deposited.

[0071] In step (6), it should be noted that since the next SiN transition layer is generally an amorphous growth structure, the columnar crystal structure of the AlSiN transition layer is difficult to grow continuously with the amorphous structure of the SiN transition layer. Therefore, the surface of the AlSiN transition layer does not need to be subjected to a crystal growth regulation process. Of course, the growth structure of the material may be different if different deposition techniques are adopted. If the SiN transition layer is a columnar crystal growth structure, in order to prevent continuous growth between the AlSiN transition layer and the SiN transition layer, after the AlSiN transition layer is deposited, its surface still needs to be subjected to a crystal growth regulation process.

[0072] In some embodiments of the present invention, in step (7), the flow rate of the argon atmosphere is 40-50 SCCM, the flow rate of the nitrogen atmosphere is 5-7 SCCM, the RF power is 300-400 W, and the deposition pressure is 3.0-4.0×10 -3 Torr, the deposition rate is 3-6nm / min. By controlling the deposition time, a SiN transition layer with a thickness of 0.1-0.6μm can be deposited.

[0073] In step (7), it should be noted that since the SiN transition layer and the Si transition layer are generally amorphous growth structures, there will be no continuous growth between the SiN transition layer and the Si transition layer, so the surface of the SiN transition layer does not need to be subjected to a crystal growth regulation process. Of course, if different deposition techniques are adopted, the growth structure of the material may be different. If the SiN transition layer and the Si transition layer are both columnar crystal growth structures, in order to prevent continuous growth between the SiN transition layer and the Si transition layer, after the SiN transition layer is deposited, its surface still needs to be subjected to a crystal growth regulation process.

[0074] In some embodiments of the present invention, in step (8), the flow rate of the argon atmosphere is 40-50 SCCM, the DC power is 300-400 W, and the deposition pressure is 3.0-4.0×10 -3 Torr, the turntable speed is 30r / min, the deposition rate is 3-6nm / min, and by controlling the deposition time, a Si transition layer with a thickness of 0.1-0.6μm can be deposited.

[0075] In step (8), it should be noted that since the Si transition layer is generally an amorphous growth structure, there will be no continuous growth between the Si transition layer and the AlN top layer, so the surface of the Si transition layer does not need to be oxidized. Of course, the growth structure of the material may be different if different deposition techniques are used. If the Si transition layer is a columnar crystal growth structure, in order to prevent continuous growth between the Si transition layer and the AlN top layer, after the Si transition layer is deposited, its surface still needs to be subjected to crystal growth control treatment.

[0076] In some embodiments of the present invention, in step (9), the flow rate of the argon atmosphere is 40-50 SCCM, the flow rate of the nitrogen atmosphere is 5-7 SCCM, the RF power is 300-400 W, the turntable speed is 30 r / min, and the deposition pressure is 3.0-4.0×10 - 3 Torr, the deposition rate is 3-6nm / min. By controlling the deposition time, the AlN top layer with a thickness of 0.1-0.6μm can be deposited.

[0077] Furthermore, the method further comprises: after the deposition is completed, the nitrogen is turned off, the arc source target power supply is turned off, the vacuum state is continued, the furnace is cooled to room temperature, and the sample is taken out, so as to obtain a non-continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating. In the embodiment of the present invention, the specific contents of the structure and use method of the magnetron sputtering coating machine belong to the conventional technology in the field and will not be repeated here.

[0078] In some embodiments of the present invention, the thickness of the Al base layer is 0.3-1.5 μm (e.g., 0.3 / 0.5 / 0.7 / 0.9 / 1.2 / 1.5 μm), the thickness of the AlN transition layer is 0.3-1.5 μm (e.g., 0.3 / 0.5 / 0.7 / 0.9 / 1.2 / 1.5 μm), and the thickness of the AlSiN transition layer is 0.3-1.5 μm (e.g., 0.3 / 0.5 / 0.7 / 0.9 / 1.2 / 1.5μm), the thickness of the SiN transition layer is 0.1-0.6μm (for example, 0.1 / 0.2 / 0.3 / 0.4 / 0.5 / 0.6μm), the thickness of the Si transition layer is 0.1-0.6μm (for example, 0.1 / 0.2 / 0.3 / 0.4 / 0.5 / 0.6μm), and the thickness of the AlN top layer is 0.1-0.6μm (for example, 0.1 / 0.2 / 0.3 / 0.4 / 0.5 / 0.6μm). The total thickness of the non-continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating is 1.2-6.3μm (for example, 1.2 / 2.1 / 3.0 / 3.9 / 5.1 / 6.3μm).

[0079] Therefore, limiting the thickness of each layer within the above range can not only provide the expected protection for the substrate, but also ensure that the coating does not have defects such as large clusters, pinholes, microcracks and falling off. The inventors found that if the thickness of the Al base layer is too small, the Al layer will not be able to fill the microscopic grooves of the substrate, and the coating will have poor adhesion. If the thickness of the Al base layer is too large, the coating surface defects will increase; if the thickness of the AlN transition layer is too small, the AlN transition layer will have poor adhesion with the Al layer and the AlSiN layer, respectively, and the coating will have poor corrosion resistance. If the thickness of the AlN transition layer is too large, it will cause excessive growth of columnar crystals, resulting in defects such as large clusters and pinholes; if the thickness of the AlSiN transition layer is too small, the AlSiN transition layer will have poor adhesion with the AlN layer and the SiN layer, respectively, resulting in poor adhesion between the coatings. If the thickness of the AlSiN transition layer is too large, it will cause excessive growth of columnar crystals, resulting in defects such as large clusters and pinholes. If the thickness of the SiN transition layer is too small, the SiN transition layer will have poor bonding with the AlSiN layer and the Si layer, resulting in poor bonding between the coatings. If the thickness of the SiN transition layer is too large, the coating surface defects will increase. At the same time, the SiN deposition rate is low, resulting in a long deposition time. If the thickness of the Si transition layer is too small, the Si transition layer will have poor bonding with the SiN layer and the AlN top layer, resulting in poor bonding between the coatings. If the thickness of the Si transition layer is too large, the coating surface defects will increase. At the same time, the Si deposition rate is low, resulting in a long deposition time and an increase in the surface temperature of the coating. If the thickness of the AlN top layer is too small, the coating will not be able to display color. If the thickness of the AlN top layer is too large, the coating surface defects will increase and the color will be confused.

[0080] The preparation, characterization and measurement instruments used in the present invention are as follows: M230 multi-target magnetron sputtering coating system, Beijing Weikai Technology Co., Ltd.; JSM7610F scanning electron microscope, JEOL Ltd.; PGSTAT302N electrochemical workstation, Metrohm; D8 ADVANCE X-ray diffractometer, Bruker, Germany; argon ion polisher, Gatan, USA.

[0081] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way. Example

[0082] This embodiment provides a method for preparing a non-continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating, the flow chart of which is as follows: Figure 2 As shown, the specific steps include:

[0083] (1) Substrate pretreatment: AZ31B magnesium alloy was selected as the substrate of sample (B-1). Sample (B-1) was rough ground, fine ground, rough polished, and fine polished to a mirror surface with sandpaper, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 min in sequence, and then dried for standby use;

[0084] A magnetron sputtering coating machine was used. The target materials were 1 Al single target with a purity of 99.9% and 1 Si single target with a purity of 99.9%. The working gases were argon with a purity of 99.999% and nitrogen with a purity of 99.999%. The sample (B-1) was placed on a turntable, and the turntable was placed in the injection chamber. The injection chamber was evacuated to a vacuum of less than 4×10 -2 Torr, the robot sent the turntable to the sputtering chamber, adjusted the turntable speed to 30r / min, the deposition chamber temperature to room temperature, and evacuated to less than 1×10 -6 After 3000 rpm, argon gas was introduced with a flow rate of 40 SCCM and a negative bias voltage of 100 W, and ion bombardment was performed for 10 min.

[0085] (2) Deposition of Al base layer: vacuum pressure is less than 1×10 -6 Torr, argon gas was introduced, the flow rate of argon atmosphere was 40 SCCM, the DC power applied was 400 W, the substrate negative bias voltage was 0 V, the turntable speed was 30 r / min, and the deposition pressure was 3.8×10 - 3 Torr, the deposition rate is 18nm / min; the Al base layer is plated, the deposition time is 45min, and the thickness of the Al base layer is 0.8μm.

[0086] (3) Crystal growth control treatment: The sample (B-1) after Al deposition as the base layer was placed in the transition chamber (sample delivery chamber), and the transition chamber was ventilated with air at 1.0×10 -1 Torr to the atmospheric pressure level, and perform exposure treatment for 5 min. Then, the exposed sample is placed into the sputtering chamber by a robot.

[0087] (4) Deposition of AlN transition layer: Wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, argon and nitrogen were introduced, the flow rate of argon atmosphere was 40 SCCM, the flow rate of nitrogen atmosphere was 12 SCCM, the DC power was 400 W, the turntable speed was 30 r / min, the substrate negative bias was 0 V, and the deposition pressure was 3.8×10 -3 Torr, the deposition rate is 10nm / min; the AlN transition layer is plated, the deposition time is 80min, and the thickness of the AlN transition layer is 0.8μm.

[0088] (5) Crystal growth control treatment: The sample (B-1) after the AlN transition layer was deposited was placed in a transition chamber (sample delivery chamber) and the transition chamber was ventilated with air at 1.0×10 -1 Torr to atmospheric pressure level, and perform exposure treatment for 5 minutes. Then, the exposed sample is placed in the sputtering chamber by a robot.

[0089] (6) Deposition of AlSiN transition layer: Wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, argon and nitrogen were introduced, the flow rate of argon atmosphere was 40 SCCM, the flow rate of nitrogen atmosphere was 12 SCCM, the DC power of Al target was 400 W, the DC power of Si target was 150 W, the negative bias voltage of substrate was 0 V, the rotation speed of turntable was 30 r / min, and the deposition pressure was 3.8×10 -3 Torr, the deposition rate is 15nm / min; the AlSiN transition layer is plated, the deposition time is 54min, and the thickness of the AlSiN transition layer is 0.8μm.

[0090] (7) Deposition of SiN transition layer: Wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, argon and nitrogen were introduced, the flow rate of argon atmosphere was 40 SCCM, the flow rate of nitrogen atmosphere was 5 SCCM, the RF power was 300 W, and the deposition pressure was 3.3×10 -3 Torr, the deposition rate is 5nm / min; the SiN transition layer is plated, the deposition time is 60min, and the thickness of the SiN transition layer is 0.3μm.

[0091] (8) Deposition of Si transition layer: Wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, argon gas was introduced, the flow rate of argon atmosphere was 40 SCCM, the RF power was 300 W, and the deposition pressure was 3.0×10 -3 Torr, the turntable speed is 30r / min, the deposition rate is 4nm / min; the Si transition layer is plated, the deposition time is 50min, and the thickness of the Si transition layer is 0.2μm.

[0092] (9) Deposition of AlN top layer: Wait until the chamber pressure is pumped down to less than 1×10 -6 Torr, argon and nitrogen were introduced, the flow rate of argon atmosphere was 40 SCCM, the flow rate of nitrogen atmosphere was 6 SCCM, the RF power was 400 W, the turntable speed was 30 r / min, and the deposition pressure was 3.5×10 -3 Torr, the deposition rate is 5nm / min; the AlN top layer is plated, the deposition time is 60min, and the thickness of the AlN top layer is 0.3μm.

[0093] (10) After the deposition is completed, turn off the nitrogen gas, turn off the target power supply, continue to maintain the vacuum state, wait for the furnace to cool to room temperature, take out the sample (B-1), and prepare the discontinuously grown AlN / Si / SiN / AlSiN on the surface of the sample (B-1) / AlN / Al multilayer gradient structure anti-corrosion coating.

[0094] For comparison, the same AZ31B magnesium alloy was used as the substrate of sample (B-2), and the above steps (1)(2)(4)(6)(7)(8)(9)(10) were repeated, omitting the crystal growth regulation step, thereby preparing a continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating on the surface of sample (B-2).

[0095] The cross-sectional FESEM morphology and EDX element observation of the samples (B-1) and (B-2) prepared in Example 1 revealed Figure 3 The morphology shown, such as Figure 3 As shown in (a), it can be seen that the AlN / Si / SiN / AlSiN / AlN / Al multilayer coating on the sample (B-2) that has not undergone crystal growth regulation treatment shows an obvious continuous columnar growth structure in the AlSiN / AlN / Al layer; Figure 3 (c) shows AlN / Si / SiN / AlSiN on sample (B-1) that has undergone crystal growth control treatment. / AlN / In the Al multilayer coating, the continuous columnar growth structure in the AlSiN / AlN / Al layer disappears, which indicates that the AlSiN / AlN / The continuous columnar growth defects between Al layers are suppressed. Figure 3 (b1)-(b4) and Figure 3 (d1)-(d4), EDX element observation shows that the color pixels of the Al element on sample (B-1) and sample (B-2) gradually decrease from the bottom of the coating to the top, and the color pixels of the Si element gradually increase from the middle of the coating to the top, which indicates that the multilayer coating is an Al and Si dual-phase element gradient structure.

[0096] In order to analyze the crystal structure of the coating, the same AZ31B magnesium alloy was used as the substrate of sample (B-3), sample (B-4), sample (B-5), sample (B-6), sample (B-7), and sample (B-8), and different coatings were plated respectively:

[0097] Repeat the above steps (1) and (4) for sample (B-3) to deposit an AlN single layer on sample (B-3);

[0098] Repeat steps (1), (2), (4) on sample (B-4) to form a continuously grown AlN / Al layer on sample (B-4);

[0099] Repeat steps (1), (2), (3), (4) on sample (B-5) to deposit a non-continuously grown AlN on sample (B-5). / Al layer;

[0100] Repeat steps (1) to (6) for sample (B-6) to deposit a single layer of AlSiN on sample (B-6);

[0101] Repeat steps (1), (2), (4), (6) on sample (B-7) to form a continuously grown AlSiN / AlN / Al layer on sample (B-7);

[0102] Repeat steps (1)(2)(3)(4)(5)(6) on sample (B-8) to deposit a non-continuously grown AlSiN / AlN / Al layer.

[0103] X-ray diffraction tests were performed on samples (B-3), sample (B-4), sample (B-5), sample (B-6), sample (B-7), and sample (B-8) prepared in Example 1. The test results are as follows: Figure 4 and Figure 5 shown.

[0104] from Figure 4 It can be seen from the graph that the AlN monolayer grows in the directions of AlN (100), (101), (102) and (112) crystal planes, and the (101) crystal plane is the optimal growth direction. The diffraction peaks of Al (111), (200), (220) and (311) crystal planes are observed in the continuously grown AlN / Al coating, and the diffraction peaks of AlN (002), (101), (102) and (112) are also detected. Compared with the AlN monolayer, the grain growth direction has less (100) crystal plane and more (002) crystal plane, and the (002) crystal plane is the optimal growth direction. According to the Scherrer formula, the average grain sizes of AlN (101) in the AlN monolayer and AlN (002) in the continuously grown AlN / Al coating are 14.5 and 18.0 nm, respectively. This confirms that the continuous growth of the AlN / Al coating causes the AlN layer to grow preferentially in the vertical direction and causes the grains in this growth direction to increase. However, after the crystal growth regulation treatment, the discontinuously grown AlN / The diffraction peaks of AlN (100), (101), (102) and (112) crystal planes in the Al coating are consistent with the grain growth direction of the AlN monolayer, and the (101) crystal plane is still the optimal growth direction. According to the Scherrer formula, the average grain size of AlN (101) in the discontinuously grown AlN / Al coating is 14.6nm. Therefore, the phase structure analysis confirms that after the crystal growth regulation treatment, the connection between the AlN / Al layers is cut off, and the continuous growth and grain growth of the AlN / Al layers are inhibited, which is a discontinuous growth structure.

[0105] from Figure 5 It can be seen that the AlSiN monolayer grows on the AlN (100) and (110) crystal planes. In the continuously grown AlSiN / AlN / Al coating, there are diffraction peaks of Al (111), (200), (220) and (311) crystal planes and diffraction peaks of AlN (002), (101), (102) and (112) crystal planes. It can be seen that the diffraction peaks of the AlSiN / AlN / Al coating are the same as those of the AlN / Al coating. At the same time, no diffraction peaks of the AlN (100) and (110) crystal planes in the AlSiN monolayer can be detected. At the same time, the average grain size of the AlN (002) crystal plane in the AlN / Al and AlSiN / AlN / Al coatings are 18.0 and 27.8 nm, respectively, which once again confirms that continuous growth occurs between the AlSiN / AlN layers and leads to grain coarsening. After the crystal growth regulation treatment, in the AlSiN / AlN / The Al coating includes diffraction peaks of Al(111), (200), (220) and (311) crystal planes, and diffraction peaks of AlN (101), (102), (112) crystal planes, as well as diffraction peaks of AlN (100) and (110) crystal planes, which are consistent with the diffraction peaks of AlN (100) and (110) crystal planes detected in the AlSiN single-layer coating. According to the Scherrer formula, the average grain size of the AlN (100) crystal plane in the AlSiN single-layer and AlSiN / AlN / Al coating is 12.4nm and 12.5nm, respectively. This indicates that after the crystal growth regulation treatment, the AlSiN / AlN / The nucleation and growth direction of the AlSiN layer in the Al coating did not change, confirming that the AlSiN / AlN / AlSiN in Al coating / The AlN layer did not grow continuously and the grain size did not increase, thus inhibiting the AlSiN / The AlN layers grow continuously, which is a discontinuous growth structure.

[0106] In order to analyze the corrosion resistance of the coating, the same AZ31B magnesium alloy was used as the substrate of sample (B-9), sample (B-10), sample (B-11), and sample (B-12), and different coatings were plated respectively:

[0107] Repeat steps (1)(2)(4)(6)(7)(8)(9)(10) on sample (B-9) and sample (B-10) respectively to prepare a continuously grown AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure anti-corrosion coating on sample (B-9) and sample (B-10);

[0108] Repeat steps (1) to (10) for sample (B-11) and sample (B-12) to prepare discontinuously grown AlN / Si / SiN / AlSiN on sample (B-11) and sample (B-12). / AlN / Al multilayer gradient structure anti-corrosion coating.

[0109] The samples (B-9) and (B-11) prepared in Example 1 were subjected to electrochemical corrosion experiments in 3.5wt% NaCl corrosion solution. The experimental results are shown in FIG. Figure 6 The electrochemical results calculated by Tafel model are shown in Table 1.

[0110] Table 1

[0111]

[0112] It can be seen that the uncoated AZ31B, the continuously grown AlN / Si / SiN / AlSiN / AlN / Al-AZ31B and the discontinuously grown AlN / Si / SiN / AlSiN / AlN / The corrosion potential values ​​of Al-AZ31B are all -1.46 V, and the corresponding corrosion current densities are 1.59×10 −4 , 3.03×10 −8 and 4.75×10 −10 A / cm 2 . The continuously grown AlN / Si / SiN / AlSiN / AlN / Al can reduce the corrosion current density of magnesium alloy by 4 orders of magnitude, and the corrosion resistance of magnesium alloy substrate is greatly improved. Through crystal growth regulation, the discontinuously grown AlN / Si / SiN / AlSiN / AlN / The corrosion current density of Al-AZ31B is from 3.03×10 −8 Further reduced to 4.75×10 −10 A / cm 2, the corrosion current density value is reduced by nearly 2 orders of magnitude again, and the corrosion resistance of the coating is greatly improved. Compared with the AZ31B magnesium alloy substrate, the discontinuously grown AlN / Si / SiN / AlSiN / AlN / The Al coating reduces the corrosion current density of the substrate from 1.59×10 −4 Reduced to 4.75×10 −10 A / cm 2 , the corrosion current density is reduced by 6 orders of magnitude, which means that the discontinuously grown AlN / Si / SiN / AlSiN / AlN / Al element gradient multilayer coating will greatly improve the service life and application range of AZ31B magnesium alloy in extreme corrosion environment. So far, there has been no report on reducing the corrosion current density of magnesium alloy by 6 orders of magnitude. At the same time, the polarization resistance (Rp) corresponding to the continuous growth and discontinuous growth coatings is 8.58×10 5 and 5.48×10 7 Ω / cm 2 , and the corresponding corrosion rates are 3.53×10 -4 and 5.52×10 -6 mm / year, which further confirms the discontinuous growth of AlN / Si / SiN / AlSiN / AlN / Excellent corrosion resistance of Al element gradient multilayer coating.

[0113] The samples (B-10) and (B-12) prepared in Example 1 were immersed in 3.5wt% NaCl corrosion solution. The experimental results are as follows: Figure 7 As shown in the figure, it can be found that after 144 hours of immersion, the continuously grown AlN / Si / SiN / AlSiN / AlN / Al-AZ31B sample has begun to partially corrode, and the surface structure of the coating has been partially destroyed, that is, after 144 hours, the sample began to corrode on a large scale; however, the discontinuously grown AlN / Si / SiN / AlSiN / AlN / The surface of the Al-AZ31B sample is still intact. After immersion for 216 hours, the continuously grown AlN / Si / SiN / AlSiN / AlN / Al-AZ31B sample has begun to show serious corrosion, the surface structure of the coating has been destroyed, black corrosion products have been generated on the surface, and the coating has basically lost its ability to protect the substrate; while the non-continuously grown AlN / Si / SiN / AlSiN / AlN / The Al-AZ31B sample is still intact. After immersion for 360h, the discontinuously grown AlN / Si / SiN / AlSiN / AlN / The Al-AZ31B sample is still intact, with a smooth surface, complete structure, and no corrosion spots, which reveals the discontinuous growth of AlN / Si / SiN / AlSiN / AlN / The Al-AZ31B sample already has super corrosion resistance.

[0114] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, characterized in that: The method comprises the steps of sequentially depositing an Al layer, a first AlN layer, an AlSiN layer, a SiN layer, a Si layer and a second AlN layer on the surface of a substrate, and also comprises the step of performing a crystal growth regulation process before the steps of depositing the first AlN layer and the AlSiN layer; The step of crystal growth regulation treatment before depositing the first AlN layer comprises at least one of exposing the Al layer deposited on the substrate in an oxygen-containing atmosphere or bombarding the Al layer with oxygen ions in an oxygen-containing atmosphere; and The step of crystal growth regulation treatment before depositing the AlSiN layer comprises at least one of exposing the AlN / Al layer deposited on the substrate in an oxygen-containing atmosphere or bombarding it with oxygen ions in an oxygen-containing atmosphere; The temperature of the crystal growth regulation treatment is room temperature to 300° C., and the crystal growth regulation treatment enables non-continuous columnar growth between the first AlN layer and the Al layer; and non-continuous columnar growth between the AlSiN layer and the first AlN layer.

2. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 1, characterized in that: The steps of depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer adopt at least one of vacuum evaporation, sputtering, arc plasma coating, ion coating and molecular beam epitaxy coating.

3. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 1 or 2, characterized in that: The step of crystal growth regulation treatment before depositing the first AlN layer comprises exposing the Al layer deposited on the substrate to an atmospheric atmosphere; and, The step of crystal growth regulation treatment before depositing the AlSiN layer comprises exposing the AlN / Al layer deposited on the substrate to an atmospheric atmosphere.

4. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 1 or 2, characterized in that: The steps of depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer are carried out by magnetron sputtering coating.

5. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 4, characterized in that: Depositing the Al layer, the first AlN layer, the AlSiN layer, the SiN layer, the Si layer and the second AlN layer comprises the following steps: (1) placing the polished substrate in a sputtering chamber of a magnetron sputtering coating machine, evacuating the chamber, and then performing ion bombardment etching in an argon atmosphere; (2) turning on a direct current power supply of an Al target in an argon atmosphere to deposit an Al layer on the surface of the substrate; (3) subjecting the deposited Al layer to a crystal growth control treatment and exposing it to an atmospheric atmosphere for more than 5 minutes; (4) turning on an Al target power supply in a mixed atmosphere of argon and nitrogen to deposit a first AlN layer on the surface of the Al layer; (5) subjecting the deposited first AlN layer to a crystal growth control treatment and exposing it to an atmospheric atmosphere for more than 5 minutes; (6) turning on the power supplies of the Al target and the Si target simultaneously in a mixed atmosphere of argon and nitrogen to deposit an AlSiN layer on the surface of the first AlN layer; (7) turning on the Si target power supply in a mixed atmosphere of argon and nitrogen to deposit a SiN layer on the surface of the AlSiN layer; (8) turning on the Si target power supply in an argon atmosphere to deposit a Si layer on the surface of the SiN layer; (9) In a mixed atmosphere of argon and nitrogen, an Al target power supply is turned on to deposit a second AlN layer on the surface of the Si layer.

6. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 1 or 2, characterized in that: After the crystal growth regulation treatment, the deposited AlN / Al layer includes AlN (100), (101), (102) and (112) crystal plane diffraction peaks; and, After the crystal growth control treatment, the deposited AlSiN / AlN / Al layer includes AlN (100) and (110) crystal plane diffraction peaks.

7. The method for preparing the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 1 or 2, characterized in that: After the crystal growth regulation treatment, the average grain size of the AlN (101) crystal plane in the deposited AlN / Al layer is 14.6 nm; and, After the crystal growth regulation treatment, the average grain size of the AlN (100) crystal plane in the deposited AlSiN / AlN / Al layer is 12.5 nm.

8. An AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating, obtained by the preparation method of the AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to any one of claims 1 to 7.

9. The AlN / Si / SiN / AlSiN / AlN / Al multilayer gradient structure coating according to claim 8, characterized in that: The thickness of the Al layer is 0.3-1.5 μm, the thickness of the first AlN layer is 0.3-1.5 μm, the thickness of the AlSiN layer is 0.3-1.5 μm, the thickness of the SiN layer is 0.1-0.6 μm, the thickness of the Si layer is 0.1-0.6 μm, and the thickness of the second AlN layer is 0.1-0.6 μm.

Citation Information

Patent Citations

  • Hardened wear-resistant and anti-corrosion colored coating on surface of magnesium alloy and preparation process of coating

    CN113151794A

  • Method for in-situ growth of ultrathin aluminum oxide protection layer on surface of wurtzite aluminum nitride-based thin film and application

    CN115725945A

  • Corrosion-resistant article coated with aluminum nitride

    US20120107613A1

  • Scratch-resistant glass or glass ceramic articles

    US20150376056A1

  • Process for modifying surfaces of nitride, and nitride having surfaces modified thereby

    US6162512A