A method for preparing conductive metal particles and conductive metal particles
Through emulsification and MOD solution processing technology, gallium-based liquid metal microspheres with uniform particle size are prepared and form a "core-shell" structure, which solves the problems of uneven particle size and oxide layer of gallium-based liquid metal microspheres and achieves high specificity. Preparation of conductive metal particles with surface area suitable for flexible electronic products.
Patent Information
- Application Number
- CN202310283767.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-15
AI Technical Summary
In the existing technology, the particle size of gallium-based liquid metal microspheres is not uniform and the presence of oxide layer leads to insulation. It is difficult to prepare metal functional microspheres with heterogeneous core-shell structure, which limits its application in flexible electronic products.
By emulsifying and drying the mixed solution of liquid metal and surfactant, liquid metal microspheres with uniform particle size are obtained, and are added to the MOD solution for vibration or ultrasonic treatment to form a "core-shell" three-dimensional petal structure. Functional metal conductive particles.
It achieves the preparation of conductive metal particles with uniform and controllable particle size and large specific surface area. The morphology is more refined, and there is no need to add additional reducing agents in the traditional electroless plating process. It can quickly generate flower-like metallic silver shells, improving the product's quality. Stability and applicability.
Smart Images

Figure CN116435005B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of conductive functional materials, and in particular to a method for preparing conductive metal particles and the conductive metal particles. Background Art
[0002] At present, the application of flexible circuits in flexible electronic products such as wearable devices, healthcare, portable electronic devices and smart sensors has attracted wide attention. However, traditional flexible circuits using rigid conductive materials (such as Cu, Ag) are prone to cracks caused by metal fatigue or small bending radius during long-term use, resulting in a decrease in electrical performance. Recently, gallium-based liquid metal has the additional advantages of high conductivity, strong ductility, excellent flexibility and non-toxicity, making it an ideal substitute for traditional metal conductors in wearable electronic products. However, at present, gallium-based liquid metal is mainly microspherized by ultrasound or mechanical stirring, which has disadvantages such as uneven particle size, and the oxide layer on the surface of liquid metal microspheres makes them insulating, which also seriously limits their applicability. At the same time, metal functional microspheres with heterogeneous core-shell structures have gained widespread attention due to their advantages such as controllable structure, size and surface morphology. However, there are still problems in the rapid and large-scale preparation of functional microspheres with heterogeneous core-shell structures. Therefore, it is of great significance to explore a technical route for preparing heterogeneous core-shell metal functional microspheres with the characteristics of uniform and controllable particle size, large specific surface area, mild preparation conditions, and easy scalable production. Summary of the invention
[0003] In view of this, it is necessary to provide a method for preparing conductive metal particles with uniform and controllable particle size and large specific surface area to address the defects existing in the prior art.
[0004] To solve the above problems, this application adopts the following technical solutions:
[0005] One of the purposes of the present application is to provide a method for preparing conductive metal particles, comprising the following steps:
[0006] The mixed solution of liquid metal and surfactant is emulsified and dried to obtain liquid metal microspheres with uniform particle size;
[0007] The liquid metal microspheres are added into a MOD (metal organic deposition) solution for oscillation or ultrasonic treatment to obtain functional metal conductive particles with a "core-shell" three-dimensional petal structure.
[0008] In some embodiments, the step of emulsifying and drying a mixed solution of liquid metal and a surfactant to obtain liquid metal microspheres with uniform particle size specifically includes the following steps:
[0009] The mixed solution obtained by mixing liquid metal and surfactant is stirred, and then the mixed solution is placed in a membrane emulsifier for emulsification, and liquid metal microspheres with different uniform particle sizes are obtained through membrane emulsification tubes with different pore sizes. The liquid metal microspheres are then vacuum dried to obtain liquid metal microspheres with uniform particle sizes.
[0010] In some of the embodiments, the working pressure of the membrane emulsifier is 0.02-0.5 MPa, the size of the membrane emulsification tube is 0.1-100 μm, the emulsification power is 500 W, and the number of cycle emulsification is 1-10 times.
[0011] It can be understood that the particle size of the liquid metal microspheres prepared in the present application is uniform and controllable, while the microspheres prepared by traditional mechanical or ultrasonic methods often have a wide particle size distribution and uncontrollable size. The present application can achieve uniform particle size control of the microspheres by regulating the size of the membrane emulsification tube.
[0012] In some of the embodiments, during the heating process of the vacuum drying, the heating time is 2-6 hours and the temperature is 65-105°C.
[0013] In some embodiments, the liquid metal is an alloy of one or more of gallium, bismuth, and indium, preferably a gallium-indium alloy.
[0014] In some of the embodiments, the mass ratio of the liquid metal to the surfactant is 1:8-1:4.
[0015] In some embodiments, the surfactant is an aqueous solution of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, stearic acid, lecithin or polyvinyl pyrrolidone.
[0016] In some embodiments, in the step of adding the liquid metal microspheres to the MOD solution for shaking or ultrasonic treatment to obtain functional metal conductive particles having a "core-shell" three-dimensional petal structure, the MOD solution is prepared by the following method:
[0017] In a light-proof condition, using a peristaltic pump, the silver nitrate solution is added to the sodium citrate solution at a volume ratio of 5:1-1:50, and dried to obtain silver citrate powder;
[0018] The silver citrate powder was added to a mixed solution of ethanol and n-butanol under light-proof conditions to obtain a MOD solution, and the MOD solution was stored at -40°C to -5°C.
[0019] In some embodiments, the peristaltic pump has a speed of 10-40 r / min.
[0020] In some of the embodiments, the mixing mass ratio of ethanol to n-butanol is 2:1-4:1.
[0021] It is understandable that since the mixing of the two will release heat, adding silver citrate will make the ink extremely unstable, so after mixing, it is subjected to circulating cooling water to keep the temperature at 5°C.
[0022] In some of the embodiments, the mass ratio of the silver citrate powder to the mixed solution of ethanol and n-butanol is 1:5-2:5.
[0023] In some of the embodiments, in the step of adding the liquid metal microspheres to the MOD solution for shaking or ultrasonic treatment to obtain functional metal conductive particles having a "core-shell" three-dimensional petal structure, the mass ratio of the liquid metal microspheres to the MOD solution is 50:1-5:1.
[0024] In some of the embodiments, in the step of adding the liquid metal microspheres to the MOD solution for shaking or ultrasonic treatment to obtain functional metal conductive particles having a "core-shell" three-dimensional petal structure, the ultrasonic rate is 100-1000W and the ultrasonic time is 10s-10min.
[0025] The second object of the present application is to provide a conductive metal particle prepared by the conductive metal particle preparation method.
[0026] This application adopts the above technical solution, and its beneficial effects are as follows:
[0027] The preparation method and conductive metal particles provided in the present application are as follows: liquid metal microspheres with uniform particle size are obtained by emulsifying and drying a mixed solution of liquid metal and surfactant, and the liquid metal microspheres are added to a MOD solution for oscillation or ultrasonic treatment to obtain functional metal conductive particles with a "core-shell" three-dimensional petal structure. The morphology of the conductive metal particles prepared in the present application can be controlled by controlling the content of the reducing agent and silver source in the MOD solution and the reaction time to obtain monodisperse liquid metal conductive silver flowers with better quality, finer morphology and high specific surface area, which has a good reference and guiding significance for the controllable synthesis of three-dimensional liquid metal nano silver flowers in the future. At the same time, compared with the traditional chemical plating process, the present application utilizes the self-reduction effect of the MOD solution, without the need to add an additional reducing agent, and combines the strong electrical replacement reaction between metal silver and gallium to quickly react and generate a flower-shaped metal silver shell layer.
[0028] In addition, the preparation method of the conductive particles provided in the present application is simple, the conditions are mild, the operation is easy, the reaction efficiency is high, and compared with pure liquid metal particles, it is more acid-resistant and alkali-resistant and can be stably stored. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0030] Figure 1 The middle left picture is an optical picture of liquid metal microspheres with uniform particle size prepared by membrane emulsification with a pore size of 10 μm as provided in Example 1, and the right picture is an optical picture of liquid metal microspheres with uniform particle size prepared by membrane emulsification with a pore size of 25 μm.
[0031] Figure 2 The SEM and EDS elemental analysis test images of the functional conductive metal particles with a "core-shell" three-dimensional petal structure prepared by membrane emulsification with a pore size of 10 μm provided in Example 1, and the reaction time was 1 min.
[0032] Figure 3 The SEM and EDS elemental analysis test images of the functional conductive metal particles with a "core-shell" three-dimensional petal structure prepared by membrane emulsification with a pore size of 10 μm provided in Example 2, and the reaction time was 2 minutes.
[0033] Specific embodiment
[0034] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0035] In the description of the present application, it should be understood that the terms "upper", "lower", "horizontal", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0036] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0037] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0038] Example 1
[0039] This embodiment 1 provides a method for preparing conductive metal particles, comprising the following steps:
[0040] (1) Weigh 46.8g of liquid metal (gallium:indium=3:2, g / g) in a 1000ml beaker at room temperature, and weigh and add 200g of 0.5wt% sodium dodecyl sulfate aqueous solution, and pre-stir the mixed solution. Then pour the mixed solution into a membrane emulsifier with a membrane emulsification tube pore size of 10μm and repeat the emulsification three times. The membrane emulsification power is 500W and the working pressure is 0.25MPa to obtain an emulsion. The emulsion is placed in a 95℃ vacuum drying oven and dried for 2h to obtain liquid metal microspheres with uniform particle size. Please refer to Figure 1 .
[0041] (2) Prepare MOD ink solution: Weigh 3.0g sodium citrate and add it to 100mL deionized water to prepare sodium citrate solution. Weigh 5.2g silver nitrate and add it to 80mL deionized water to prepare silver nitrate solution, and avoid light. Use a peristaltic pump to add the silver nitrate solution to the sodium citrate solution at a speed of 20r / min, dry it in the dark for 8h, and obtain silver citrate powder. Mix 3.59g ethanol with 1.72g n-butanol, circulate cooling water to keep it at a constant temperature of 5℃ and add 1g silver citrate, stir for 0.5h, and avoid light during the process to obtain a particle-free silver citrate ink.
[0042] (3) Liquid metal microspheres were added to the MOD solution for ultrasonic treatment (the mass ratio of liquid metal microspheres to MOD solution was 10:1), the ultrasonic power was 1000 W, the ultrasonic time was 1 min, and functional metal conductive particles with a "core-shell" three-dimensional petal structure were obtained by rapid reaction. The morphology of the conductive particles is as follows: Figure 2 shown.
[0043] Example 2
[0044] This embodiment 2 provides a method for preparing conductive metal particles, comprising the following steps:
[0045] (1) Weigh 46.8g of liquid metal (gallium: indium = 3:2, g / g) in a 1000mL beaker at room temperature, and weigh and add 200g of 0.5wt% sodium dodecyl sulfate aqueous solution, and pre-stir the mixed solution. Then pour the mixed solution into a membrane emulsifier with a membrane emulsification tube size of 10μm and repeat the emulsification three times. The membrane emulsification power is 500W and the working pressure is 0.25MPa to obtain an emulsion. The emulsion is placed in a 95℃ vacuum drying oven and dried for 2h to obtain liquid metal microspheres with uniform particle size.
[0046] (2) Prepare MOD ink solution: Weigh 3.0g sodium citrate and add it to 100mL deionized water to prepare sodium citrate solution. Weigh 5.2g silver nitrate and add it to 80mL deionized water to prepare silver nitrate solution, and avoid light. Use a peristaltic pump to add the silver nitrate solution to the sodium citrate solution at 20r / min, dry it in the dark for 8h, and obtain silver citrate powder. Mix 3.59g ethanol with 1.72g n-butanol, circulate cooling water to keep it at a constant temperature of 5°C, add 1g silver citrate, stir for 0.5h, and avoid light during the process to obtain a particle-free silver citrate ink.
[0047] (3) Liquid metal microspheres were added to the MOD solution for ultrasonication (the mass ratio of liquid metal microspheres to MOD solution was 10:1), the ultrasonic power was 100 W, the ultrasonic time was 2 min, and functional metal conductive particles with a "core-shell" three-dimensional petal structure were obtained by rapid reaction. The morphology of the conductive particles is as follows: Figure 3 Picture.
[0048] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
[0049] It can be understood that the technical features of the above-described embodiments can be arbitrarily combined. In order to make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0050] The above are only preferred embodiments of the present application, and only specifically describe the technical principles of the present application. These descriptions are only for explaining the principles of the present application and cannot be interpreted as limiting the scope of protection of the present application in any way. Based on the explanation here, any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application, and other specific embodiments of the present application that can be associated with the technicians in this field without creative work, should be included in the scope of protection of the present application.
Claims
1. A method for preparing conductive metal particles, characterized in that: The specific steps are: emulsifying and drying a mixed solution of liquid metal and surfactant to obtain liquid metal microspheres with uniform particle size, wherein the mass ratio of the liquid metal to the surfactant is 1:8-1:4; Adding the liquid metal microspheres into a MOD solution and subjecting it to ultrasonic treatment to obtain functional metal conductive particles having a "core-shell" three-dimensional petal structure; In the step of emulsifying and drying the mixed solution of liquid metal and surfactant to obtain liquid metal microspheres with uniform particle size, the specific steps are: The mixed solution obtained by mixing the liquid metal and the surfactant is stirred, and then the mixed solution is placed in a membrane emulsifier for emulsification, and liquid metal microspheres with different uniform particle sizes are obtained through membrane emulsification tubes with different pore sizes, and then the liquid metal microspheres are vacuum dried to obtain liquid metal microspheres with uniform particle sizes; The working pressure of the membrane emulsifier is 0.02-0.5 Mpa, the size of the membrane emulsification tube is 0.1-100 μm, the emulsification power is 500 W, and the number of cyclic emulsification times is 1-10 times; The surfactant is a 0.5 wt% aqueous solution of sodium dodecyl sulfate; The liquid metal is a gallium-indium alloy; In the step of adding the liquid metal microspheres to the MOD solution for ultrasonic treatment to obtain functional metal conductive particles having a "core-shell" three-dimensional petal structure, the MOD solution is prepared by the following method: In a light-proof condition, using a peristaltic pump, the silver nitrate solution is added to the sodium citrate solution at a volume ratio of 5:1-1:50, and dried to obtain silver citrate powder; Keeping the condition of avoiding light, adding the silver citrate powder to a mixed solution of ethanol and n-butanol to obtain a MOD solution, wherein the mixed mass ratio of ethanol to n-butanol is 2:1-4:1; The mass ratio of the liquid metal microspheres to the MOD solution is 50:1-5:1; The ultrasonic rate is 100-1000 W, and the ultrasonic time is 10 s-10 min.
2. The method for preparing conductive metal particles according to claim 1, characterized in that: During the heating process of the vacuum drying, the heating time is 2-6 h and the temperature is 65-105°C.
3. The method for preparing conductive metal particles according to claim 1, characterized in that: The MOD solution was stored at -40°C to -5°C.
4. The method for preparing conductive metal particles according to claim 1, characterized in that: The peristaltic pump speed is 10-40 r / min.
5. A conductive metal particle, characterized in that: The conductive metal particles are prepared by the method for preparing the conductive metal particles according to any one of claims 1 to 4.