A trace metal ion adsorbent in NMP system
The GO-EPSSS adsorbent synthesized through emulsion polymerization and radial micro-centrifugal adsorption bed technology solves the problem of difficulty in removing trace metal ions and easy dissolution in the NMP system, achieving efficient metal ion adsorption and low-cost industrial-grade purification.
Patent Information
- Application Number
- CN202310574596.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-22
AI Technical Summary
Existing adsorbents are difficult to effectively remove trace metal ions in NMP systems, and are easily eluted in organic solvents, resulting in low metal ion removal efficiency.
The GO-EPSSS adsorbent was synthesized by emulsion polymerization. By introducing sodium p-styrene sulfonate and divinylbenzene, the amphiphilicity and sulfonic acid group of GO were used to achieve the adsorption of metal ions, and then it was shaped and loaded into the diameter. In the micro-centrifugal adsorption bed, the contact probability between metal ions and adsorbent is increased through radial micro-flow.
It achieves efficient adsorption of trace metal ions in the NMP system, reaching SEMI C8 standards (the concentration of each metal ion is less than 1 ppb), and regenerates the adsorbent through acidification, saving operating costs.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis of trace metal ion adsorbing materials in organic matter, and in particular relates to a trace metal ion adsorbent in an NMP system. Background Art
[0002] Ultra-clean and high-purity reagents, also known as wet chemicals, play a key role in the processing and preparation of integrated circuits. They are mainly used to clean chips and silicon wafers. With the development of microelectronics technology, the integration of circuits is getting higher and higher, and the corresponding line width is getting smaller and smaller, and the requirements for ultra-high purity reagents are getting higher and higher. Ultra-high purity reagents mainly include general wet electronic chemicals and functional wet electronic chemicals. General wet electronic chemicals mainly include: organic solvents, acids and alkalis; functional wet electronic chemicals mainly include: etching solutions, developers, stripping solutions and diluents. Among them, N-Methyl pyrrolidone (NMP) is one of the most widely used electronic grade organic solvents due to its strong solubility, good biodegradability, and stable chemical properties. It is called the "universal solvent."
[0003] High concentration of metal ions in ultra-high purity reagents can cause breakdown of silicon wafers and damage their service life. Therefore, it is necessary to remove impurities from ultra-high purity reagents. The purification of ultra-high purity reagents in industry mainly includes distillation, sub-boiling distillation and adsorption. Among them, the adsorption method has the advantages of flexible production operation, easy control and low energy consumption, and has great industrial prospects.
[0004] GO contains hydrophilic groups such as carboxyl and hydroxyl groups, as well as lipophilic groups such as benzene rings, so it has amphiphilic properties and can be used as an emulsifier for emulsion polymerization. At the same time, the structure of GO has excellent adsorption properties for a variety of metal ions. For alkali metal ions (sodium ions, potassium ions, etc.) that are difficult to remove, they can be removed by introducing sulfonic acid groups in the form of ion exchange. The present invention uses emulsion polymerization to obtain the adsorbent GO-EPSSS from sodium styrene sulfonate, GO and divinylbenzene, and introduces it into a styrene suspension polymerization system for molding to obtain a granular adsorbent. Through the construction of multiple adsorption sites, it has excellent adsorption capacity for metal ions in the NMP system. At the same time, the use of a radial microgravity adsorption bed to achieve the adsorption of trace metal ions in NMP can effectively increase the contact probability between trace metal ions and the active sites of the adsorbent, and has good application prospects. Summary of the invention
[0005] The purpose of the present invention is to provide an adsorbent for trace metal ions in an NMP system, so as to overcome the problems that the existing adsorbents are difficult to adsorb trace metal ions and are easily dissolved in organic solvents, and to provide a more efficient adsorbent for removing trace metal ions in the NMP system.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing a trace metal ion adsorbent in an NMP system comprises the following steps:
[0008] (1) Dissolve GO in water to prepare GO solution, add sodium p-styrene sulfonate and stir to dissolve; add divinylbenzene dropwise under high-speed stirring, control the addition time to not exceed 3 minutes, and then ultrasonically vibrate until the solution is uniform in color; under nitrogen protection, keep the temperature at 40°C, add initiator ammonium persulfate and dispersant polyvinyl pyrrolidone, raise the temperature to 80°C, and react for 6 hours;
[0009] (2) Add acetone to break the emulsion, then wash repeatedly by centrifugation with acetone and deionized water, and freeze-dry to obtain GO-EPSSS;
[0010] (3) Add GO-EPSSS to styrene and disperse by ultrasonic to obtain a GO-EPSSS dispersion; add gelatin to deionized water and stir to dissolve at 40°C to obtain a gelatin solution; drop the GO-EPSSS dispersion into the gelatin solution, then add the crosslinking agent divinylbenzene and the initiator benzoyl peroxide, keep the mixture at 40°C for 30 min, heat to 85°C for polymerization for 6 h, heat to 95°C for blending for 4 h, repeatedly wash with ethanol and deionized water, and dry to obtain molded GO-EPSSS;
[0011] (4) The formed GO-EPSSS is placed in a chromatography column, and hydrochloric acid and tetramethylammonium hydroxide solution are repeatedly passed through the column three times, followed by soaking in hydrochloric acid, and then centrifugally washed with deionized water and freeze-dried to obtain the trace metal ion adsorbent in the NMP system.
[0012] In the solution of step (1), the GO concentration is 0.5-2 g / L, the concentration of sodium p-styrene sulfonate is 0.1-0.3 mol / L, the molar ratio of divinylbenzene to sodium p-styrene sulfonate is 1:0.8-1.2; the high-speed stirring time is 0.5-2 h, the ultrasonic oscillation time is 1-2 h; the insulation time is 0.5-1 h; the molar ratio of ammonium persulfate to sodium p-styrene sulfonate is 1:90-110, and the mass of polyvinyl pyrrolidone is 2-5% of the mass of divinylbenzene.
[0013] The amount of acetone used in step (2) for demulsification is 3-5 times the volume of the reaction solution.
[0014] In step (3), the mass ratio of GO-EPSSS to styrene is 3-20:100, the mass ratio of gelatin to water is 1-2:100, the mass ratio of water to styrene is 10-20:1, the mass ratio of divinylbenzene to styrene is 5-30:100, and the mass ratio of benzoyl peroxide to styrene is 0.1-1:100.
[0015] The concentration of the hydrochloric acid and tetramethylammonium hydroxide solution in step (4) is 1 mol / L.
[0016] The particle size of the trace metal ion adsorbent in the NMP system prepared by the method described above is 0.5-5 mm.
[0017] The adsorbent is loaded into a radial micro-centrifugal adsorption bed, the axial to radial length ratio of the radial micro-centrifugal adsorption bed is 1:10-20, the rotation speed of the radial micro-centrifugal adsorption bed is 1-5 rpm, NMP enters from the center of the radial micro-centrifugal adsorption bed, and is discharged from the radial edge of the adsorption bed.
[0018] The adsorbent and its radial microcentrifugal adsorption bed process are suitable for purifying trace metal ion impurities (sodium ions, potassium ions, zinc ions and magnesium ions, etc.) in industrial-grade NMP to meet the requirements of SEMI C8, that is, the concentration of each metal ion is less than 1 ppb.
[0019] The beneficial effects of the present invention are:
[0020] The present invention adopts emulsion polymerization to construct an adsorbent of GO, sodium p-styrene sulfonate and divinylbenzene copolymer. In this system, the amphiphilicity of GO is used as an emulsifier for the reaction. At the same time, it can be activated by an initiator and can also be used as a monomer for the reaction. The introduction of sodium p-styrene sulfonate provides a -SO3H functional group, and the sulfonic acid group can react with Na + , K + GO contains a large number of carboxyl groups, which can also undergo replacement reactions with metal ions. GO has a large π conjugated system and oxygen-containing heteroatom functional groups, which can coordinate with divalent and high-valent metals, thereby achieving the purpose of removing metal ions. The adsorbent is introduced into a styrene suspension polymerization system for molding, which increases the particle size while retaining the adsorption sites. The adsorbent involved in the present invention effectively solves the problem of the difficulty of traditional adsorbents in removing trace metal ions by constructing multiple adsorption sites, and has an adsorption effect on most trace metal ions.
[0021] The present invention uses the adsorbent GO-EPSSS obtained by emulsion polymerization for adsorption of trace metal ions in the NMP system, and has excellent adsorption performance. The formed adsorbent is loaded into a radial micro-centrifugal adsorption bed to continuously purify industrial-grade NMP. NMP enters from the center of the radial micro-centrifugal adsorption bed and then diffuses to both sides. In this process, the amount of adsorbent gradually increases, and the metal ion content in NMP gradually decreases. The radial flow effectively increases the residence time of NMP and the contact probability of metal ions and adsorbent. In this process, the adsorbent can be regenerated by acidification, which effectively saves operating costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The structure diagram of the radial microcentrifugal adsorption bed is shown in FIG. The markings in the figure are: liquid inlet pipe 1, shell 2, upper rotating disk 3, liquid separation hole 4, bolt 5, rotating disk liquid outlet 6, lower rotating disk 7, liquid outlet hole 8, rotating shaft 9.
[0023] Figure 2 This is a physical picture of the molded adsorbent and a schematic diagram of the diameter test. DETAILED DESCRIPTION
[0024] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0025] Example 1
[0026] (1) 100 mg of GO was dissolved in 100 mL of water to form a GO solution, which was stirred for 2 h. Then 5 g of sodium p-styrene sulfonate was added and stirred until completely dissolved. Then, 3 g of divinylbenzene was added dropwise to the aqueous solution at 10,000 r / min for no more than 3 minutes. After stirring, the solution was ultrasonically shaken for a period of time until the entire solution was uniform in color.
[0027] (2) The above solution was transferred to a 250 mL three-necked flask and kept at 40 °C for 2 h under nitrogen protection. Then, 0.2 g of ammonium persulfate and 0.1 g of polyvinyl pyrrolidone were dissolved in 5 mL of water and added dropwise to the three-necked flask. The temperature was then raised to 80 °C and the reaction was allowed to proceed for 6 h.
[0028] (3) Add an appropriate amount of acetone to the solution obtained by the reaction to demulsify, use acetone and deionized water to wash repeatedly by centrifugation, and dry it by freeze drying. After drying, put it into a chromatography column, use 1 M hydrochloric acid and 1 M tetramethylammonium hydroxide solution to pass the column for three times, and finally soak the column with hydrochloric acid, wash it by centrifugation with deionized water, and freeze dry it to obtain the final product, named GO-EPSSS.
[0029] (4) Take 100 mg of GO-EPSSS and add it to 2 g of styrene, and ultrasonicate for 2 h until it is completely dissolved; take 0.5 g of gelatin and add it to 30 mL of water, stir at 40 °C until it is completely dissolved; add 0.5 divinylbenzene to the mixture of GO-EPSSS and styrene, and then add the mixture to the water dissolved with gelatin, and preheat it at 40 °C for 1 h; after preheating, add 0.5 g of benzoyl peroxide, heat it to 80 °C and keep it for 6 h; then heat it to 95 °C and keep it for 3 h. After the reaction is completed, cool it naturally, use ethanol and ultrapure water to filter and wash it, and finally obtain the formed GO-EPSSS, and then use 1M hydrochloric acid and 1M tetramethylammonium hydroxide solution to pass through the column for three times, and finally soak the column with hydrochloric acid, centrifuge and wash it with deionized water, and freeze-dry to obtain the final product.
[0030] Example 2
[0031] (1) 50 mg of GO was dissolved in 100 mL of water to form a GO solution, which was stirred for 2 h. Then, 2.5 g of sodium p-styrene sulfonate was added and stirred until it was completely dissolved. Then, 2.4 g of divinylbenzene was added dropwise to the aqueous solution at 10,000 r / min for no more than 3 minutes. After stirring, the solution was ultrasonically shaken for a period of time until the entire solution was uniform in color.
[0032] (2) The above solution was transferred to a 250 mL three-necked flask and kept at 40 °C for 2 h under nitrogen protection. Then, 0.18 g of ammonium persulfate and 0.05 g of polyvinyl pyrrolidone were dissolved in 5 mL of water and added dropwise to the three-necked flask. The temperature was then raised to 80 °C and the reaction was allowed to proceed for 6 h.
[0033] (3) Add an appropriate amount of acetone to the solution obtained by the reaction to demulsify, use acetone and deionized water to wash repeatedly by centrifugation, and dry it by freeze drying. After drying, put it into a chromatography column, use 1 M hydrochloric acid and 1 M tetramethylammonium hydroxide solution to pass the column for three times, and finally soak the column with hydrochloric acid, wash it by centrifugation with deionized water, and freeze dry it to obtain the final product, named GO-EPSSS.
[0034] (4) Take 100 mg of GO-EPSSS and add it to 0.5 g of styrene, and ultrasonicate for 2 h until it is completely dissolved; take 0.05 g of gelatin and add it to 5 mL of water, and stir at 40 °C until it is completely dissolved; add 0.025 g of divinylbenzene to the mixture of GO-EPSSS and styrene, and then add the mixture to the water dissolved with gelatin, and preheat it at 40 °C for 1 h; after preheating, add 0.005 g of benzoyl peroxide, heat it to 80 °C and keep it for 6 h; then heat it to 95 °C and keep it for 3 h. After the reaction is completed, it is cooled naturally, and it is filtered and washed with ethanol and ultrapure water to finally obtain the formed GO-EPSSS, and then it is treated with 1M hydrochloric acid and 1M tetramethylammonium hydroxide solution for three times, and finally the column is soaked with hydrochloric acid, centrifuged and washed with deionized water, and freeze-dried to obtain the final product.
[0035] Example 3
[0036] (1) 200 mg of GO was dissolved in 100 mL of water to form a GO solution, which was stirred for 2 h. Then 7.5 g of sodium p-styrene sulfonate was added and stirred until it was completely dissolved. Then, 3.6 g of divinylbenzene was added dropwise to the aqueous solution at 10,000 r / min for no more than 3 minutes. After stirring, the solution was ultrasonically shaken for a period of time until the entire solution was uniform in color.
[0037] (2) The above solution was transferred to a 250 mL three-necked flask and kept at 40 °C for 2 h under nitrogen protection. Then, 0.22 g of ammonium persulfate and 0.18 g of polyvinyl pyrrolidone were dissolved in 5 mL of water and added dropwise to the three-necked flask. The temperature was then raised to 80 °C and the reaction was continued for 6 h.
[0038] (3) Add an appropriate amount of acetone to the solution obtained by the reaction to demulsify, use acetone and deionized water to wash repeatedly by centrifugation, and dry it by freeze drying. After drying, put it into a chromatography column, use 1 M hydrochloric acid and 1 M tetramethylammonium hydroxide solution to pass the column for three times, and finally soak the column with hydrochloric acid, wash it by centrifugation with deionized water, and freeze dry it to obtain the final product, named GO-EPSSS.
[0039] (4) Take 100 mg of GO-EPSSS and add it to 3 g of styrene, and ultrasonicate for 2 h until it is completely dissolved; take 1.2 g of gelatin and add it to 60 mL of water, and stir at 40 °C until it is completely dissolved; add 1.0 g of divinylbenzene to the mixture of GO-EPSSS and styrene, and then add the mixture to the water in which the gelatin is dissolved, and preheat it at 40 °C for 1 h; after preheating, add 0.03 g of benzoyl peroxide, heat it to 80 °C and keep it for 6 h; then heat it to 95 °C and keep it for 3 h. After the reaction is completed, it is cooled naturally, and it is filtered and washed with ethanol and ultrapure water to finally obtain the formed GO-EPSSS, and then it is treated with 1M hydrochloric acid and 1M tetramethylammonium hydroxide solution for three times, and finally the column is soaked with hydrochloric acid, centrifuged and washed with deionized water, and freeze-dried to obtain the final product.
[0040] Application Example 1
[0041] The NMP obtained after industrial-grade distillation was purified using a radial microcentrifugal adsorption bed, and the changes in its main metal ion impurities were detected.
[0042] The main process is: the NMP raw liquid enters the radial microcentrifugal adsorption bed from the liquid inlet pipe 1, and is evenly dispersed under the action of the liquid separation hole 4. Under the action of centrifugal force, NMP diffuses outward and flows through the area filled with adsorbent, and as NMP flows, the amount of adsorbent gradually increases. After NMP flows through the adsorbent area, it will flow into the shell, flow through the liquid outlet hole 8 to leave the adsorption bed, and complete the adsorption. The adsorption bed has a diameter of 2 m and a height of 0.25 m. The diameter of the part filled with adsorbent is 1.8 m and the height is 0.2 m. The rotation speed is 10 rpm, and the flow rate of NMP is 20 mL / min. After running for 12 hours, the metal ions were detected, and the results are shown in the following table:
[0043] Table 1 Metal ion concentrations in NMP after 12 h adsorption in radial microcentrifuge adsorption bed
[0044]
[0045] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing a trace metal ion adsorbent in an NMP system, characterized in that: The following steps are involved: (1) Dissolve GO in water to prepare GO solution, add sodium p-styrene sulfonate and stir to dissolve; add divinylbenzene dropwise under high-speed stirring, control the addition time to not exceed 3 minutes, and then ultrasonically vibrate until the solution is uniform in color; under nitrogen protection, keep the temperature at 40°C, add initiator ammonium persulfate and dispersant polyvinyl pyrrolidone, raise the temperature to 80°C, and react for 6 hours; (2) Add acetone to break the emulsion, then wash repeatedly by centrifugation with acetone and deionized water, and freeze-dry to obtain GO-EPSSS; (3) Add GO-EPSSS to styrene and disperse by ultrasonic to obtain a GO-EPSSS dispersion; add gelatin to deionized water and stir to dissolve at 40°C to obtain a gelatin solution; drop the GO-EPSSS dispersion into the gelatin solution, add divinylbenzene as a crosslinker and benzoyl peroxide as an initiator, keep the mixture at 40°C for 30 min, heat to 85°C for polymerization for 6 h, heat to 95°C for blending for 4 h, repeatedly wash with ethanol and deionized water, and dry to obtain molded GO-EPSSS; (4) The formed GO-EPSSS is placed in a chromatography column, and hydrochloric acid and tetramethylammonium hydroxide solution are repeatedly passed through the column three times, followed by soaking in hydrochloric acid, and then centrifugally washed with deionized water and freeze-dried to obtain the trace metal ion adsorbent in the NMP system.
2. The method according to claim 1, characterized in that: In the solution of step (1), the GO concentration is 0.5-2 g / L, the concentration of sodium p-styrene sulfonate is 0.1-0.3 mol / L, the molar ratio of divinylbenzene to sodium p-styrene sulfonate is 1:0.8-1.2; the high-speed stirring time is 0.5-2 h, the ultrasonic oscillation time is 1-2 h; the insulation time is 0.5-1 h; the molar ratio of ammonium persulfate to sodium p-styrene sulfonate is 1:90-110, and the mass of polyvinyl pyrrolidone is 2-5% of the mass of divinylbenzene.
3. The method according to claim 1, characterized in that: The amount of acetone used in step (2) for demulsification is 3-5 times the volume of the reaction solution.
4. The method according to claim 1, characterized in that: In step (3), the mass ratio of GO-EPSSS to styrene is 5-20:100, the mass ratio of gelatin to deionized water is 1-2:100, the mass ratio of deionized water to styrene is 2-5:1, the mass ratio of divinylbenzene to styrene is 5-30:100, and the mass ratio of benzoyl peroxide to styrene is 0.1-1:
100.
5. The method according to claim 1, characterized in that: In step (4), the concentrations of hydrochloric acid and tetramethylammonium hydroxide solution are both 1 mol / L.
6. An adsorbent for trace metal ions in NMP system prepared by the method according to claim 1, characterized in that: The adsorbent particle size is 0.5-5 mm.
7. An application of a trace metal ion adsorbent in an NMP system prepared by the method according to claim 1, characterized in that: The adsorbent is loaded in a radial micro-centrifugal adsorption bed, the axial to radial length ratio of the radial micro-centrifugal adsorption bed is 1:10-20, the rotation speed of the radial micro-centrifugal adsorption bed is 1-5 rpm, NMP enters from the center of the radial micro-centrifugal adsorption bed, and is discharged from the radial edge of the adsorption bed.
Citation Information
Patent Citations
Preparation method of magnetic porous adsorbent by suspension polymerization
CN103588919A
Method for preparing high specific capacitance reduction-oxidation graphene
CN104003377A