A method for recycling waste catalyst

By treating the waste supported hydrogenation catalyst with alkaline and acidic treatment, combined with the gelation reaction of organic solvents and aluminum acidic alkaline solutions, a new hydrocracking catalyst with good hydrogenation and cracking properties was prepared, solving the problem of waste catalyst recycling Utilize the complexity and value of unused issues to achieve efficient recycling and low-cost production.

CN116440942BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202210008427.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-06
Publication Date
2024-10-01
Estimated Expiration
2042-01-06

AI Technical Summary

Technical Problem

Existing technology cannot effectively treat and recover metal pollutants in discarded supported hydrogenation catalysts, and the process is complex and fails to fully utilize the value of the catalyst.

Method used

After oil removal, carbon removal, crushing and screening, alkaline and acidic solution treatment is used to recover the molybdenum and nickel-containing solution, and the organic solvent and aluminum acidic alkaline solution are combined to perform a gelling reaction to form a new hydrocracking catalyst carrier, and pass Impregnating active metal components to prepare new hydrocracking catalysts with good hydrogenation and cracking properties.

Benefits of technology

Efficient recycling of waste catalysts is achieved, production costs are reduced, and the comprehensive utilization value of the catalyst is improved. The new catalyst obtained is suitable for the hydrocracking treatment of inferior raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116440942B_ABST
    Figure CN116440942B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for recycling waste catalysts. The method comprises: (1) removing oil, carbon, crushing and screening the waste supported hydrocracking catalyst; (2) using alkaline solution for alkali treatment to obtain a molybdenum-containing aqueous solution and a nickel-aluminum-silicon-containing solid residue; (3) using an acidic solution for acid treatment to obtain a nickel-containing aqueous solution and a silicon-aluminum material containing a Y-type molecular sieve; (4) adding an organic solvent and a silicon-aluminum material containing a Y-type molecular sieve into a reactor, adding an aluminum-containing acidic solution and an aluminum-containing alkaline solution, performing a first gelling reaction, and then alternately adding an aluminum-containing acidic solution and an aluminum-containing alkaline solution in sequence, swinging to form a gel, aging, and obtaining a catalyst carrier; (5) using a solution containing an active metal component to impregnate the catalyst carrier, drying, and calcining to obtain a novel hydrocracking catalyst. The hydrocracking catalyst obtained by the method has good hydrogenation and cracking performance and better raw material adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recycling a waste catalyst, and in particular to a method for recycling a waste supported hydrocracking catalyst to prepare a novel hydrocracking catalyst. Background Art

[0002] In the past, the main method of disposing of waste supported hydrogenation catalysts was landfill. However, China currently produces more than 100,000 tons of waste supported hydrogenation catalysts each year, and it will continue to grow rapidly at a rate of 4.4% per year. It is urgent to develop efficient treatment and clean recycling technology for toxic metal pollutants in waste supported hydrogenation catalysts.

[0003] CN107723468A discloses a waste catalyst comprehensive utilization system. The system includes a de-oiling furnace, a rotary kiln, a four-stage countercurrent device, a stirring tank I, a plate-frame filter I, a precipitation tank I, a plate-frame filter II, a stirring tank II, a centrifuge I, an ion exchange resin, an extraction device, a back extraction device, a precipitation tank II, a centrifuge II and a washing tank. The process can effectively recycle the useful components in the waste catalyst of residual oil hydrogenation to obtain products such as industrial steam, nickel aluminum powder, ammonium metavanadate, high-purity molybdic acid, anhydrous sodium sulfate and distilled water, and high-purity molybdic acid can be obtained without multiple separation processes, but the process is complicated.

[0004] CN104628032B discloses a method for preparing high-purity ammonium metavanadate from waste catalysts. The method comprises: collecting waste catalyst leachate by leaching, filtering the leachate and then entering the ion exchange dephosphorization system, using resin to adsorb phosphorus, and adsorbing phosphorus in the waste catalyst leachate; after dephosphorization, the molybdenum-vanadium solution enters the ion exchange system, and uses resin to adsorb molybdenum to separate molybdenum and vanadium; pumping the vanadium-containing mother liquor after dephosphorization and molybdenum separation into a vanadium precipitation tank, and performing weak alkaline ammonium salt vanadium precipitation to obtain a high-purity ammonium metavanadate product. The invention has the characteristics of short process, simple process, energy saving and environmental protection, high efficiency, and low cost, but it fails to make the best use of materials and fails to fully tap the value of waste hydrogenation catalysts. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for recycling waste catalysts. The method uses waste supported hydrocracking catalysts as raw materials to prepare new hydrocracking catalysts. The method has the characteristics of simple preparation process, high metal recovery rate, low processing cost, etc., and the obtained hydrocracking catalyst has good hydrogenation and cracking performance and better raw material adaptability.

[0006] The present invention provides a method for recycling waste catalysts, comprising:

[0007] (1) removing oil and carbon from the waste supported hydrocracking catalyst, and then crushing and screening it;

[0008] (2) treating the powder after screening in step (1) with an alkaline solution to obtain an aqueous solution containing molybdenum and a solid residue containing nickel, aluminum and silicon;

[0009] (3) using an acidic solution to acid-treat the nickel-aluminum-silicon-containing solid residue obtained in step (2) to obtain a nickel-containing aqueous solution and a silicon-aluminum material containing a Y-type molecular sieve;

[0010] (4) adding an organic solvent and the silicon-aluminum material containing Y molecular sieve obtained in step (3) into a reaction kettle, stirring, adding an aluminum-containing acidic solution and an aluminum-containing alkaline solution, adjusting the pH value to perform a first gelation reaction, and then alternately adding the aluminum-containing acidic solution and the aluminum-containing alkaline solution in sequence, performing swing gelation, aging, and obtaining a catalyst carrier;

[0011] (5) The catalyst carrier obtained in step (4) is impregnated with a solution containing active metal components, and the solution is dried and calcined to obtain a novel hydrocracking catalyst.

[0012] In the method of the present invention, in step (1), based on the weight of the waste supported hydrocracking catalyst, the content of catalyst solids is 70% to 90%, and the content of petroleum fractions is 10% to 30%.

[0013] In the method of the present invention, in step (1), the active metals supported by the waste supported hydrocracking catalyst include molybdenum and nickel. The support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve, and the mass content of Al2O3 is 5% to 95% and the mass content of Y-type molecular sieve is 5% to 95% based on the mass of the support.

[0014] In the method of the present invention, in step (1), the oil removal is generally performed by extraction. The organic solvent used for the extraction is at least one of toluene, petroleum ether, ethanol, etc., the extraction temperature is 80-110° C., and the extraction time is 5-60 hours.

[0015] In the method of the present invention, in step (1), the carbon removal can be carried out by roasting, the roasting temperature is 500-700°C, preferably 600-650°C, and the roasting time is 2-48h, preferably 5-24h. After deoiling and carbon removal, the weight content of nickel oxide in the waste supported hydrocracking catalyst is 2%-10%, the weight content of molybdenum oxide is 15%-50%, and the weight content of carbon is less than 1%.

[0016] In the method of the present invention, in step (1), the particle size of the powder obtained after the pulverization and sieving is 200 to 400 meshes, preferably 300 to 400 meshes.

[0017] In the method of the present invention, in step (2), the alkaline solution is a solution of one or more of ammonia water, urea, ammonium carbonate, ammonium bicarbonate, etc., and its concentration is 5g / 100mL to 100g / 100mL, preferably 10g / 100mL to 90g / 100mL; the liquid-to-solid mass ratio of the alkaline solution to the powder screened in step (1) is 1:1 to 50:1, preferably 2:1 to 45:1.

[0018] In the method of the present invention, in step (2), the conditions of the alkali treatment are as follows: temperature of 100-400°C, preferably 150-350°C, treatment time of 0.5-4.0h, preferably 0.5-3.0h, pressure of 5-20MPa, preferably 5-15MPa, and heating rate to the treatment temperature of 5-25°C / min, preferably 5-10°C / min.

[0019] In the method of the present invention, in step (2), after the alkali treatment, the molybdenum-containing aqueous solution and the solid residue containing nickel, aluminum and silicon are obtained by conventional filtration, washing and drying. Preferably, after the alkali treatment, the leaching rate of molybdenum oxide is 90% to 98%, preferably 95% to 98%. The leaching rate of molybdenum oxide is the ratio of the mass of molybdenum in the molybdenum-containing aqueous solution to the mass of molybdenum in the waste supported hydrocracking catalyst, calculated as molybdenum oxide.

[0020] In the method of the present invention, in step (3), the acidic solution is a solution of one or more of oxalic acid, carbonic acid, EDTA, acetic acid, sulfurous acid, etc., and its concentration is 5g / 100mL to 100g / 100mL, preferably 10g / 100mL to 90g / 100mL. The liquid-to-solid mass ratio of the acidic compound in the acidic solution to the solid residue containing nickel, silicon, and aluminum obtained in step (2) is 1:1 to 50:1, preferably 2:1 to 45:1.

[0021] In the method of the present invention, in step (3), the conditions of the acid treatment are as follows: temperature is 100-400°C, preferably 150-350°C, treatment time is 0.5-4.0h, preferably 0.5-3.0h, reaction pressure is 5-20MPa, preferably 5-15MPa, heating rate is 5-25°C / min, preferably 5-10°C / min. Preferably, after the acid treatment, the leaching rate of nickel oxide is 90%-98%, preferably 95%-98%. The leaching rate of nickel oxide is the ratio of the mass of nickel in the nickel-containing aqueous solution to the mass of nickel in the waste supported hydrocracking catalyst, calculated as nickel oxide.

[0022] In the method of the present invention, in step (3), after the acid treatment, conventional filtration, washing and drying are performed to obtain a nickel-containing aqueous solution and a silicon-aluminum material containing a Y-type molecular sieve.

[0023] In the method of the present invention, in step (3), the SiO2 / Al2O3 molar ratio of the silicon-aluminum material containing the Y molecular sieve is 2:1 to 50:1, preferably 2:1 to 25:1, and the pore volume is 0.4 to 0.8 mL·g -1 ; Specific surface area is 650~750m 2 ·g -1 ; The pore diameter can be ≮5nm, preferably 5-7nm.

[0024] In the method of the present invention, in step (4), the organic solvent is one or more of alkanes, alkenes, organic alcohols, organic acids, etc., and further, the alkanes are preferably at least one of pentane, hexane, dodecane, etc.; the alkenes are preferably at least one of pentene, hexene, etc.; the organic alcohol is selected from at least one of organic monohydric alcohols and organic polyhydric alcohols, preferably at least one of n-hexanol, n-heptanol, pentaerythritol, glycerol, trimethylolethane, xylitol, sorbitol, etc.; the organic acid is selected from at least one of aliphatic or aromatic carboxylic acids, such as benzoic acid, etc. The amount of the organic solvent added is 1 / 5 to 1 / 2 of the actual effective use volume of the reactor.

[0025] In the method of the present invention, in step (4), the concentration of the aluminum-containing alkaline salt solution is 10-20 g / 100 mL in terms of aluminum oxide; and the concentration of the aluminum-containing acidic salt solution is 5-10 g / 100 mL in terms of aluminum oxide.

[0026] In the method of the present invention, in step (4), the pH of the first gelling step is 7.0 to 9.0, the time is 3 to 15 minutes, and the temperature is 50 to 100° C., preferably 70 to 100° C.;

[0027] The time of each gelation in the swing gelation is 3 to 15 minutes, and the temperature of the swing gelation is 50 to 100° C., preferably 70 to 100° C. The pH value of the swing gelation is adjusted to 2.0 to 3.0 during acid gelation and to 10.0 to 11.0 during alkaline gelation. The number of swings is 2 to 8 times, preferably 3 to 5 times. The entire gelation process is carried out under stirring, and the stirring rate is 20 to 500 rad / min, preferably 20 to 300 rad / min.

[0028] In the method of the present invention, in step (4), the aging conditions are as follows: pH value is 7.0-9.0, temperature is 50-100° C., preferably 70-100° C., time is 0.5-2.5 h, preferably 1.0-2.0 h.

[0029] In the method of the present invention, in step (4), after aging, conventional filtration, drying and calcination are performed to obtain a catalyst carrier.

[0030] In the method of the present invention, in step (5), the active metal is selected from one or more metal elements of Group VIII and / or Group VIB, preferably one or more of tungsten, molybdenum, cobalt or nickel.

[0031] In the method of the present invention, in step (5), the impregnation solution containing active metals can be the molybdenum-containing aqueous solution and the nickel-containing aqueous solution recovered in step (2) and step (3).

[0032] In the method of the present invention, in step (5), the impregnation can be carried out by a conventional impregnation method in the art, such as equal volume impregnation, etc. The drying temperature is 100-200°C, preferably 120-150°C, the drying time is 2-10 hours, the roasting temperature is 300-800°C, preferably 350-550°C, and the roasting time is 2.0-5.0 hours, preferably 2.0-4.0 hours.

[0033] The novel hydrocracking catalyst obtained by the present invention has R as the catalyst particle radius, the silicon aluminum material containing the Y-type molecular sieve is distributed in the range from the center to R / 2 to 2R / 3, and the aluminum oxide is distributed in the range from R / 2 to 2R / 3 to R.

[0034] The novel hydrocracking catalyst of the present invention has the following properties: pore volume of 1.5 to 2.0 mL·g -1 ; Specific surface area is 300~450m 2 ·g -1 The pore size may be ≮10 nm, preferably 15 to 25 nm; the particle size distribution is as follows: the proportion of particles with a diameter of less than 100 μm is 0.5% to 1%, the proportion of particles with a diameter of 100 to 200 μm is 2% to 5%, and the proportion of particles with a diameter of more than 200 μm is 90% to 95%.

[0035] In the novel hydrocracking catalyst, the carrier content is 65% to 95% by weight of the catalyst, the content of active metal in oxide form is 5% to 35% by weight of the catalyst. Further, the content of Group VIII metal in oxidation state is 3% to 30% by weight of the catalyst, and the content of Group VIB metal in oxide form is 0.5% to 5%.

[0036] The present invention also provides an application of the obtained novel hydrocracking catalyst, which is to apply the novel hydrocracking catalyst to the hydrocracking treatment of heavy and inferior raw materials.

[0037] The heavy and inferior raw materials are at least one of diesel, wax oil, residual oil, coal tar, coal liquefied oil and the like.

[0038] Compared with the prior art, the present invention has the following advantages:

[0039] The method of the present invention firstly treats the recovered waste hydrocracking catalyst with an acidic solution and an alkaline solution, and obtains a silicon-aluminum material retaining the complete structure of the Y molecular sieve on the basis of recovering molybdenum and nickel solutions. The material in this specific state is used as a crystal nucleus, first mixed with an organic solvent, and an alumina carrier material is formed on the outer layer of the crystal nucleus by pH swing neutralization. The prepared catalyst has excellent hydrocracking performance and is suitable for processing inferior raw materials.

[0040] The method of the present invention realizes the recycling of waste hydrocracking catalysts, greatly reduces the production cost of the catalysts, and improves the comprehensive utilization value of the waste catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the SEM image of the new hydrocracking catalyst A obtained in Example 1. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with the examples, but it should be understood that the protection scope of the present invention is not limited by the examples. In the present invention, unless otherwise clearly stated, percentages and percentage contents are all based on mass.

[0043] The SEM images of the present invention are measured using a field emission scanning electron microscope (JSM7500F), electron gun type: cold field emission gun, acceleration voltage: 0.1 kW to 30 kW, resolution: 1.0 nm (secondary electrons), 3.0 nm (backscattered electrons), magnification: 25 to 1,000,000.

[0044] Example 1

[0045] A waste supported hydrocracking catalyst containing 30% oil (the support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve, and the mass content of Al2O3 is 80% and the mass content of Y-type molecular sieve is 20% based on the mass of the support) is extracted with petroleum ether at 100°C for 48 hours and then calcined at 600°C for 10 hours. The obtained waste supported hydrocracking catalyst has a MoO3 weight content of 25.5%, a NiO weight content of 8.5%, and a carbon content of ≤0.9%. It is then crushed and sieved to obtain a powder of 300-400 mesh.

[0046] An ammonium carbonate solution with a concentration of 25g / 100mL and the above-mentioned 100g powder are mixed evenly in a liquid-solid mass ratio of 10:1 and added into an autoclave. The temperature is raised to 200°C at a heating rate of 5°C / min. The reaction pressure is 10.0MPa and the constant temperature time is 2.5h. After filtering, washing until the washing liquid is neutral and drying at 150°C for 2h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum are obtained, wherein the leaching rate of MoO3 is 98%.

[0047] An oxalic acid solution with a concentration of 20g / 100mL and the above-mentioned 75g of nickel-silicon-aluminum solid residue were mixed uniformly in a liquid-solid mass ratio of 10:1 and added into an autoclave. The temperature was raised to 250°C at a heating rate of 10°C / min. The reaction pressure was 13.0MPa and the constant temperature time was 3h. After filtering, washing until the washing liquid was neutral and drying at 120°C for 4h, a nickel-containing solution and a silicon-aluminum material A containing Y molecular sieve were obtained. The properties thereof are shown in Table 1, wherein the leaching rate of NiO was 97.8%.

[0048] The above 50g of silicon-aluminum material containing Y molecular sieve was added to the reactor, and 5L of n-hexane was added to the reactor, the stirring rate was controlled to 150rad / min, and then a sodium aluminate solution with a concentration of 15g / 100mL was added at a rate of 5mL / min, and an aluminum sulfate solution with a concentration of 5g / 100mL was added at the same time, the pH value was controlled to 7.5, the temperature was 75°C, and the addition of the sodium aluminate solution was stopped after the neutralization time of 5min; the aluminum sulfate solution with a concentration of 5g / 100mL was continued to be added, and the addition was stopped when the pH value was controlled to 3.0, and it was stabilized for 5min; then a sodium aluminate solution with a concentration of 15g / 100mL was added, and the addition was stopped when the pH value was controlled to 11.0, and it was stabilized for 5min, and then the aluminum sulfate solution and the sodium aluminate solution were added as above, and after swinging 3 times, the aging pH value was adjusted to 9.0, the aging temperature was controlled to 100°C, and the aging time was 2h, and then filtered, dried at 150°C for 5h, and calcined at 500°C for 4h to obtain the desired catalyst carrier. The obtained carrier was impregnated with the molybdenum-containing solution and the nickel-containing solution obtained above, dried at 120° C. for 3 h, and calcined at 450° C. for 3 h to obtain a novel hydrocracking catalyst A, the properties of which are shown in Table 2.

[0049] Example 2

[0050] A waste supported hydrocracking catalyst containing 25% oil (the support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve, and the mass content of Al2O3 is 95% and the mass content of Y-type molecular sieve is 5% based on the mass of the support) is extracted at 90°C for 50 hours with a mixed solution of petroleum ether and ether in a volume ratio of 1:1, and then calcined at 650°C for 5 hours. The obtained waste supported hydrocracking catalyst has a MoO3 weight content of 24.7%, a NiO weight content of 8.8%, and a carbon content of ≤0.8%. It is then crushed and sieved to obtain a powder of 300-400 meshes.

[0051] An ammonia solution with a concentration of 30g / 100mL and the above-mentioned 250g powder are mixed evenly at a liquid-to-solid mass ratio of 15:1 and added to an autoclave. The temperature is raised to 280°C at a heating rate of 10°C / min. The reaction pressure is 13.0MPa and the constant temperature time is 3.0h. After filtering, washing until the washing liquid is neutral and drying at 140°C for 4h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum are obtained, wherein the leaching rate of MoO3 is 97%.

[0052] An EDTA solution with a concentration of 15g / 100mL and the above-mentioned 186g of nickel-containing silicon-aluminum solid residue were mixed uniformly in a liquid-solid mass ratio of 18:1 and added into an autoclave. The temperature was raised to 200°C at a heating rate of 10°C / min. The reaction pressure was 15.0MPa and the constant temperature time was 2.5h. After filtering, washing until the washing liquid was neutral and drying at 150°C for 3h, a nickel-containing solution and a silicon-aluminum material B containing Y molecular sieve were obtained. The properties thereof are shown in Table 1, wherein the leaching rate of NiO was 98%.

[0053] The above 100g of silicon-aluminum material containing Y molecular sieve was crushed and added to the reactor, and 10L of n-hexanol was added to the reactor, the stirring rate was controlled at 200rad / min, and then a sodium aluminate solution with a concentration of 12g / 100mL was added at a rate of 10mL / min, and an aluminum sulfate solution with a concentration of 10g / 100mL was added at the same time, the pH value was controlled to 8.5, the temperature was 90°C, and the addition of the sodium aluminate solution was stopped after the neutralization time of 5min; the aluminum sulfate solution with a concentration of 10g / 100mL was continued to be added, and the addition was stopped when the pH value was controlled to 2.0, and it was stabilized for 5min; then a sodium aluminate solution with a concentration of 12g / 100mL was added, and the addition was stopped when the pH value was controlled to 10.0, and it was stabilized for 5min, and then the aluminum sulfate solution and the sodium aluminate solution were added as above, and the aging pH value was adjusted to 8.5 after swinging 3 times, the aging temperature was controlled to 100°C, and the aging time was 1.5h, and then filtered, dried at 200°C for 2h, The desired catalyst carrier was obtained by calcining at 500°C for 4 hours. The carrier was impregnated with the molybdenum-containing solution and the nickel-containing solution obtained above, dried at 150°C for 2 hours, and calcined at 550°C for 4 hours to obtain a novel hydrocracking catalyst B, the properties of which are shown in Table 2.

[0054] Example 3

[0055] A waste supported hydrocracking catalyst containing 28% oil (the support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve. Based on the mass of the support, the mass content of Al2O3 is 70%, and the mass content of Y-type molecular sieve is 30%) is extracted with toluene at 110°C for 32 hours and then calcined at 630°C for 12 hours. The obtained waste supported hydrocracking catalyst has a MoO3 weight content of 26.9%, a NiO weight content of 9.6%, and a carbon content of ≤1.0%. The catalyst is then crushed and sieved to obtain a powder of 300-400 mesh.

[0056] A 45g / 100mL urea solution and the above 500g powder were mixed evenly at a liquid-solid mass ratio of 20:1 and added into an autoclave. The temperature was raised to 300°C at a heating rate of 8°C / min. The reaction pressure was 15.0MPa and the constant temperature time was 2.0h. After filtering and washing until the washing liquid was neutral and drying at 140°C for 4h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum were obtained, wherein the leaching rate of MoO3 was 97.9%.

[0057] An acetic acid solution with a concentration of 30g / 100mL and the above-mentioned 379g of nickel-containing silicon-aluminum solid residue were mixed uniformly at a liquid-solid mass ratio of 20:1 and added into an autoclave, and the temperature was raised to 270°C at a heating rate of 10°C / min, the reaction pressure was 14.6MPa, the constant temperature time was 2.0h, and after filtering, washing until the washing liquid was neutral, and drying at 150°C for 5h, a nickel-containing solution and a silicon-aluminum material C containing a Y molecular sieve were obtained, and their properties are shown in Table 1, wherein the leaching rate of NiO was 97.9%.

[0058] The above 300g of silicon-aluminum material containing Y molecular sieve is added to the reactor, and 20L of styrene is added to the reactor, the stirring rate is controlled to 190rad / min, and then a sodium aluminate solution with a concentration of 20g / 100mL is added at a rate of 25mL / min, and an aluminum sulfate solution with a concentration of 8g / 100mL is added at the same time, the pH value is controlled to 8.0, the reaction temperature is 95°C, and the addition of the sodium aluminate solution is stopped after the neutralization time of 5min; the aluminum sulfate solution with a concentration of 8g / 100mL is continued to be added, and the addition is stopped when the pH value is controlled to 2.0, and it is stabilized for 5min; then a sodium aluminate solution with a concentration of 20g / 100mL is added, and the addition is stopped when the pH value is controlled to 10.5, and it is stabilized for 5min, and then the aluminum sulfate solution and the sodium aluminate solution are added as above, and the swing is repeated for 3 times. After the aging pH value was adjusted to 7.5, the aging temperature was controlled to 95°C, and the aging time was 2.0h, and then the catalyst carrier was obtained by filtration, drying at 150°C for 3h, and calcining at 550°C for 5h. The carrier was impregnated with the molybdenum-containing solution and the nickel-containing solution obtained above, dried at 140°C for 5h, and calcined at 400°C for 3h to obtain a novel hydrocracking catalyst C, the properties of which are shown in Table 2.

[0059] Example 4

[0060] A waste supported hydrocracking catalyst containing 20% ​​oil (the support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve. Based on the mass of the support, the mass content of Al2O3 is 45%, and the mass content of Y-type molecular sieve is 55%) is extracted at 110°C for 36 hours using toluene and petroleum ether in a volume ratio of 1:1. The extracted catalyst is then calcined at 650°C for 8 hours. The weight content of MoO3 in the obtained waste supported hydrocracking catalyst is 27.5%, the weight content of NiO is 9.5%, and the carbon content is ≤0.8%. The catalyst is then crushed and sieved to obtain a powder of 300-400 mesh.

[0061] An ammonium carbonate solution with a concentration of 20g / 100mL and the above-mentioned 200g powder are mixed evenly in a liquid-to-solid mass ratio of 8:1 and added into an autoclave. The temperature is raised to 220°C at a heating rate of 10°C / min. The reaction pressure is 11.0MPa and the constant temperature time is 2.0h. After filtering, washing until the washing liquid is neutral and drying at 150°C for 3h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum are obtained, wherein the leaching rate of MoO3 is 98%.

[0062] An oxalic acid solution with a concentration of 25g / 100mL and the above-mentioned 175g of nickel-silicon-aluminum solid residue were mixed uniformly in a liquid-solid mass ratio of 8:1 and added into an autoclave, and the temperature was raised to 300°C at a heating rate of 8°C / min. The reaction pressure was 15.0MPa, and the constant temperature time was 2.5h. After filtering, washing until the washing liquid was neutral, and drying at 180°C for 2h, a nickel-containing solution and a silicon-aluminum material D containing a Y molecular sieve were obtained. The properties thereof are shown in Table 1, wherein the leaching rate of NiO was 97.5%.

[0063] The above 150g of the silicon-aluminum material containing the Y molecular sieve was added to the reactor, and 10L of hexane was added to the reactor, the stirring rate was controlled to 150rad / min, and then a sodium aluminate solution with a concentration of 20g / 100mL was added at a rate of 10mL / min. At the same time, add aluminum sulfate solution with a concentration of 10g / 100mL, control the pH value to 7.0, the reaction temperature to 85℃, and stop adding sodium aluminate solution after neutralization time of 5min; continue to add aluminum sulfate solution with a concentration of 10g / 100mL, control the pH value to 3.2, stop adding, and stabilize for 5min; then add sodium aluminate solution with a concentration of 20g / 100mL, control the pH value to 11.5, stop adding, and stabilize for 5min, then add aluminum sulfate solution and sodium aluminate solution as above, swing 4 times, adjust the aging pH value to 9.0, control the aging temperature to 90℃, and after aging time of 3h, filter, dry at 120℃ for 5h, and roast at 500℃ for 3h to obtain the desired catalyst carrier. The carrier obtained by impregnating the above-obtained molybdenum-containing solution and nickel-containing solution, drying at 120℃ for 3h, and roasting at 450℃ for 3h, a new hydrocracking catalyst D is obtained, and its properties are shown in Table 2.

[0064] Example 5

[0065] A waste supported hydrocracking catalyst containing 25% oil (the support of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve, and the mass content of Al2O3 is 60% and the mass content of Y-type molecular sieve is 40% based on the mass of the support) is extracted at 110°C for 38 hours using toluene and ether in a volume ratio of 1:1, and then calcined at 620°C for 8 hours. The obtained waste supported hydrocracking catalyst has a MoO3 weight content of 26.5%, a NiO weight content of 8.9%, and a carbon content of ≤0.9%. It is then crushed and sieved to obtain a powder of 300-400 mesh.

[0066] An ammonium carbonate solution with a concentration of 40g / 100mL and the above 300g powder are mixed evenly in a liquid-to-solid mass ratio of 5:1 and added into an autoclave. The temperature is raised to 250°C at a heating rate of 10°C / min. The reaction pressure is 13.0MPa and the constant temperature time is 2.0h. After filtering, washing until the washing liquid is neutral and drying at 130°C for 4h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum are obtained, wherein the leaching rate of MoO3 is 97.5%.

[0067] An oxalic acid solution with a concentration of 15g / 100mL and the above-mentioned 269g of nickel-containing silicon-aluminum solid residue were mixed uniformly at a liquid-solid mass ratio of 20:1 and added into an autoclave, and the temperature was raised to 300°C at a heating rate of 8°C / min, the reaction pressure was 15.0MPa, the constant temperature time was 2.5h, and after filtering, washing until the washing liquid was neutral, and drying at 150°C for 5h, a nickel-containing solution and a silicon-aluminum material E containing a Y molecular sieve were obtained. The properties thereof are shown in Table 1, wherein the leaching rate of NiO was 98.0%.

[0068] The above 100g of silicon-aluminum material containing Y molecular sieve was added to the reactor, and 15L of dodecane was added to the reactor, the stirring rate was controlled to 120rad / min, and then a sodium aluminate solution with a concentration of 16g / 100mL was added at a rate of 6mL / min, and an aluminum sulfate solution with a concentration of 15g / 100mL was added at the same time, the pH value was controlled to 7.0, the reaction temperature was 85°C, and the addition of the sodium aluminate solution was stopped after the neutralization time of 5min; the aluminum sulfate solution with a concentration of 15g / 100mL was continued to be added, and the addition was stopped when the pH value was controlled to 3.0, and it was stabilized for 5min; then a sodium aluminate solution with a concentration of 16g / 100mL was added, and the addition was stopped when the pH value was controlled to 11.5, and it was stabilized for 5min, and then the aluminum sulfate solution and the sodium aluminate solution were added as above, and the aging pH value was adjusted to 10.0 after swinging 3 times, and the aging temperature was controlled to 95°C. After the aging time of 3.0h, it was filtered, dried at 170°C for 2h, and dried at 450°C. The desired catalyst carrier was obtained by calcining for 4 hours. The carrier was impregnated with the molybdenum-containing solution and the nickel-containing solution obtained above, dried at 120°C for 3 hours, and calcined at 450°C for 3 hours to obtain a novel hydrocracking catalyst E, the properties of which are shown in Table 2.

[0069] Comparative Example 1

[0070] 350g of purchased Y molecular sieve (its properties are shown in Table 1) was added to the reactor, and 15L of pure water was added to the reactor, the stirring rate was controlled to 190rad / min, the reaction temperature was 95°C, and then the addition rate of the sodium aluminate solution with a concentration of 20g / 100mL was controlled to be 25mL / min, and at the same time, an aluminum sulfate solution with a concentration of 8g / 100mL was added, the pH value was controlled to be 8.0, and the addition of the sodium aluminate solution was stopped after the neutralization time of 5min; the aluminum sulfate solution with a concentration of 8g / 100mL was continued to be added, and the addition was stopped when the pH value was controlled to 2.0, and it was stabilized for 5min; then a sodium aluminate solution with a concentration of 20g / 100mL was added, and the addition was stopped when the pH value was controlled to 10.5, and it was stabilized for 5min, and then the aluminum sulfate solution and the sodium aluminate solution were added as above, and after swinging 3 times, the aging pH value was adjusted to 7.5, the aging temperature was controlled to 95°C, and the aging time was 2.0h, and then filtered, dried at 150°C for 3h, The desired catalyst carrier was obtained by calcining at 550°C for 3h. The carrier was impregnated with the molybdenum-containing solution and the nickel-containing solution obtained above, dried at 140°C for 5h, and calcined at 400°C for 3h to obtain a hydrocracking catalyst F, the properties of which are shown in Table 2.

[0071] Comparative Example 2

[0072] The waste supported hydrocracking catalyst containing 28% oil (same as in Example 3) was extracted with toluene at 110°C for 32h and then calcined at 630°C for 12h. The obtained waste supported hydrocracking catalyst had a MoO3 weight content of 26.9%, a NiO weight content of 9.6%, and a carbon content of ≤1.0%. The catalyst was then crushed and sieved to obtain a powder of 300-400 mesh.

[0073] A 45g / 100mL urea solution and the above 500g powder were mixed evenly at a liquid-solid mass ratio of 20:1 and added into an autoclave. The temperature was raised to 300°C at a heating rate of 8°C / min. The reaction pressure was 15.0MPa and the constant temperature time was 2.0h. After filtering and washing until the washing liquid was neutral and drying at 140°C for 4h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum were obtained, wherein the leaching rate of MoO3 was 97.9%.

[0074] An acetic acid solution with a concentration of 30g / 100mL and the above-mentioned 379g of nickel-containing silicon-aluminum solid residue were mixed uniformly at a liquid-solid mass ratio of 20:1 and added into an autoclave, and the temperature was raised to 270°C at a heating rate of 10°C / min, the reaction pressure was 14.6MPa, the constant temperature time was 2.0h, and after filtering, washing until the washing liquid was neutral, and drying at 150°C for 5h, a nickel-containing solution and a silicon-aluminum material C containing a Y molecular sieve were obtained, and their properties are shown in Table 1, wherein the leaching rate of NiO was 97.9%.

[0075] The obtained molybdenum-containing solution and nickel-containing solution were impregnated into the obtained silicon-aluminum material G containing Y molecular sieve, dried at 140° C. for 5 h, and calcined at 400° C. for 3 h to obtain a hydrocracking catalyst G, the properties of which are shown in Table 2.

[0076] Comparative Example 3

[0077] The waste supported hydrocracking catalyst containing 28% oil (same as in Example 3) was extracted with toluene at 110°C for 32h and then calcined at 630°C for 12h. The obtained waste supported hydrocracking catalyst had a MoO3 weight content of 26.9%, a NiO weight content of 9.6%, and a carbon content of ≤1.0%. The catalyst was then crushed and sieved to obtain a powder of 300-400 mesh.

[0078] A 45g / 100mL urea solution and the above 500g powder were mixed evenly at a liquid-solid mass ratio of 20:1 and added into an autoclave. The temperature was raised to 300°C at a heating rate of 8°C / min. The reaction pressure was 15.0MPa and the constant temperature time was 2.0h. After filtering and washing until the washing liquid was neutral and drying at 140°C for 4h, a molybdenum-containing solution and a solid residue containing nickel, silicon and aluminum were obtained, wherein the leaching rate of MoO3 was 97.9%.

[0079] An acetic acid solution with a concentration of 30g / 100mL and the above-mentioned 379g of nickel-containing silicon-aluminum solid residue were mixed uniformly at a liquid-solid mass ratio of 20:1 and added into an autoclave, and the temperature was raised to 270°C at a heating rate of 10°C / min. The reaction pressure was 14.6MPa, and the constant temperature time was 2.0h. After filtering, washing until the washing liquid was neutral, and drying at 150°C for 5h, a nickel-containing solution and a silicon-aluminum material H containing a Y molecular sieve were obtained. The properties thereof are shown in Table 1, wherein the leaching rate of NiO was 97.9%.

[0080] The above 300g of the silicon-aluminum material containing Y molecular sieve was added to the reactor, and 20L of pure water was added to the reactor to control the stirring rate to 190rad / min, and then a sodium aluminate solution with a concentration of 20g / 100mL was added at a rate of 25mL / min, and an aluminum sulfate solution with a concentration of 8g / 100mL was added at the same time, the pH value was controlled to 8.0, the reaction temperature was 95°C, and the neutralization time was 5min Then stop adding sodium aluminate solution; continue to add aluminum sulfate solution with a concentration of 8g / 100mL, stop adding when the pH value is controlled to 2.0, and stabilize for 5min; then add sodium aluminate solution with a concentration of 20g / 100mL, stop adding when the pH value is controlled to 10.5, and stabilize for 5min, then add aluminum sulfate solution and sodium aluminate solution as above, and adjust the aging pH value to 7.5 after swinging 3 times, control the aging temperature to 95℃, and after aging for 2.0h, filter, dry at 150℃ for 3h, and roast at 550℃ for 5h to obtain the desired catalyst carrier. The carrier obtained by impregnating the above-obtained molybdenum-containing solution and nickel-containing solution, drying at 140℃ for 5h, and roasting at 400℃ for 3h, obtains hydrocracking catalyst H, and its properties are shown in Table 2.

[0081] Table 1

[0082]

[0083] Table 2 Properties of the novel hydrocracking catalysts obtained in Examples and Comparative Examples

[0084]

[0085] Example 6

[0086] The above catalysts A, B, C, D and E of the present invention were subjected to an activity evaluation test. The test adopted a series process flow, and the properties of the raw oil used are shown in Table 3. The operating conditions are as follows: hydrogen partial pressure 15.4MPa, hydrogen oil volume ratio 1200:1, liquid hourly volume space velocity 1.2h -1 , the nitrogen content of the hydrorefined oil was controlled to be 10-15 μg / g. The catalyst activity test results are shown in Table 4.

[0087] Comparative Example 4

[0088] The comparative example catalysts F, G and H were subjected to activity evaluation tests. The evaluation conditions were the same as those in Example 6. The catalyst activity test results are shown in Table 4.

[0089] Table 3 Raw oil properties

[0090] Iranian Vacuum Gas Oil <![CDATA[Density (20 °C) / (g / cm 3 )]]> 0.9089 Distillation range, ℃ 303~547 Nitrogen content / wt% 0.135 Sulfur content / wt% 1.65 Aromatics / wt% 38.5 Pour point, ℃ 35

[0091] Table 4 Catalyst activity evaluation results

[0092]

[0093]

[0094] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. Any simple modifications, equivalent changes and modifications made to the above exemplary embodiments should fall within the scope of protection of the present invention.

Claims

1. A method for recycling waste catalysts, characterized in that: The method comprises: (1) removing oil and carbon from the waste supported hydrocracking catalyst, and then crushing and screening it; (2) treating the powder after screening in step (1) with an alkaline solution to obtain an aqueous solution containing molybdenum and a solid residue containing nickel, aluminum and silicon; (3) using an acidic solution to acid-treat the nickel-aluminum-silicon-containing solid residue obtained in step (2) to obtain a nickel-containing aqueous solution and a silicon-aluminum material containing a Y-type molecular sieve; (4) adding an organic solvent and the silicon-aluminum material containing Y molecular sieve obtained in step (3) into a reaction kettle, stirring, adding an aluminum-containing acidic solution and an aluminum-containing alkaline solution, adjusting the pH value to perform a first gelation reaction, and then alternately adding the aluminum-containing acidic solution and the aluminum-containing alkaline solution in sequence, performing swing gelation, aging, and obtaining a catalyst carrier; (5) impregnating the catalyst support obtained in step (4) with a solution containing active metal components, drying and calcining to obtain a novel hydrocracking catalyst; In step (1), the carrier of the waste supported hydrocracking catalyst includes Al2O3 and Y-type molecular sieve.

2. The method according to claim 1, characterized in that In step (1), the active metals carried by the waste supported hydrocracking catalyst include molybdenum and nickel; based on the mass of the carrier of the waste supported hydrocracking catalyst, the mass content of Al2O3 is 5% to 95%, and the mass content of Y-type molecular sieve is 5% to 95%.

3. The method according to claim 1, characterized in that In step (1), the oil removal is carried out by extraction, the organic solvent used for the extraction is at least one of toluene, petroleum ether and ethanol, the extraction temperature is 80-110° C., and the extraction time is 5-60 hours.

4. The method according to claim 1, characterized in that In step (1), the carbon removal is carried out by roasting, the roasting temperature is 500-700° C., and the roasting time is 2-48 hours.

5. The method according to claim 1, 3 or 4, characterized in that: In step (1), the weight content of nickel oxide in the waste supported hydrocracking catalyst after oil and carbon removal is 2% to 10%, the weight content of molybdenum oxide is 15% to 50%, and the weight content of carbon is less than 1%; the particle size of the powder obtained after crushing and sieving is 200 to 400 meshes.

6. The method according to claim 1, characterized in that In step (2), the alkaline solution is a solution of one or more of ammonia water, urea, ammonium carbonate, and ammonium bicarbonate, and its concentration is 5g / 100mL to 100g / 100mL; the liquid-to-solid mass ratio of the alkaline solution to the powder screened in step (1) is 1:1 to 50:

1.

7. The method according to claim 6, characterized in that In step (2), the concentration of the alkaline solution is 10 g / 100 mL to 90 g / 100 mL; the liquid-to-solid mass ratio of the alkaline solution to the powder screened in step (1) is 2:1 to 45:

1.

8. The method according to claim 1, characterized in that In step (2), the conditions of the alkali treatment are as follows: temperature of 100-400°C, treatment time of 0.5-4.0h, pressure of 5-20MPa, and heating rate to the treatment temperature of 5-25°C / min; after alkali treatment, the leaching rate of molybdenum oxide is 90%-98%.

9. The method according to claim 8, characterized in that In step (2), the conditions of the alkali treatment are as follows: temperature of 150-350°C, treatment time of 0.5-3.0h, pressure of 5-15MPa, and heating rate to the treatment temperature of 5-10°C / min; after alkali treatment, the leaching rate of molybdenum oxide is 95%-98%.

10. The method according to claim 1, characterized in that In step (3), the acidic solution is a solution of one or more of oxalic acid, carbonic acid, EDTA, acetic acid, and sulfurous acid, and its concentration is 5g / 100mL to 100g / 100mL; the liquid-to-solid mass ratio of the acidic compound in the acidic solution to the solid residue containing nickel, silicon, and aluminum obtained in step (2) is 1:1 to 50:

1.

11. The method according to claim 10, characterized in that In step (3), the concentration of the acidic solution is 10 g / 100 mL to 90 g / 100 mL; the liquid-to-solid mass ratio of the acidic compound in the acidic solution to the nickel-silicon-aluminum-containing solid residue obtained in step (2) is 2:1 to 45:

1.

12. The method according to claim 1, characterized in that In step (3), the conditions of the acid treatment are as follows: temperature of 100-400° C., treatment time of 0.5-4.0 h, reaction pressure of 5-20 MPa, and heating rate of 5-25° C. / min; after acid treatment, the leaching rate of nickel oxide is 90%-98%.

13. The method according to claim 12, characterized in that In step (3), the conditions of the acid treatment are as follows: temperature of 150-350° C., treatment time of 0.5-3.0 h, reaction pressure of 5-15 MPa, and heating rate of 5-10° C. / min; after acid treatment, the leaching rate of nickel oxide is 95%-98%.

14. The method according to claim 1, characterized in that In step (3), the SiO2 / Al2O3 molar ratio of the silicon-aluminum material containing Y molecular sieve is 2:1-50:1, and the pore volume is 0.4-0.8 mL·g -1 ; Specific surface area is 650~750m 2 ·g -1 ; Pore diameter ≮5nm.

15. The method according to claim 14, characterized in that In step (3), the SiO2 / Al2O3 molar ratio of the silicon-aluminum material containing Y molecular sieve is 2:1 to 25:1, and the pore size is 5 to 7 nm.

16. The method according to claim 1, characterized in that In step (4), the organic solvent is one or more of alkanes, olefins, organic alcohols, and organic acids.

17. The method according to claim 16, characterized in that The alkane is at least one of pentane, hexane and dodecane; the olefin is at least one of pentene and hexene; the organic alcohol is at least one of organic monohydric alcohol and organic polyhydric alcohol; the organic acid is at least one of aliphatic or aromatic carboxylic acids.

18. The method according to claim 17, characterized in that The organic alcohol is at least one of n-hexanol, n-heptanol, pentaerythritol, glycerol, trimethylolethane, xylitol and sorbitol.

19. The method according to claim 1, characterized in that In step (4), the concentration of the aluminum-containing alkaline solution is 10 to 20 g / 100 mL in terms of aluminum oxide; and the concentration of the aluminum-containing acidic solution is 5 to 10 g / 100 mL in terms of aluminum oxide.

20. The method according to claim 1, characterized in that In step (4), the pH of the first gelling step is 7.0 to 9.0, the time is 3 to 15 minutes, and the temperature is 50 to 100° C.; and / or, The time of each gelation in the swing gelation is 3 to 15 minutes, the temperature of the swing gelation is 50 to 100° C., the pH value of the swing gelation is adjusted to 2.0 to 3.0 during acidic gelation, and the pH value is adjusted to 10.0 to 11.0 during alkaline gelation, the number of swings is 2 to 8 times, and the entire gelation process is carried out under stirring at a stirring rate of 20 to 500 rad / min.

21. The method according to claim 20, characterized in that In step (4), the temperature of the first gelling step is 70-100°C.

22. The method according to claim 1, characterized in that In step (4), the aging conditions are as follows: pH value is 7.0-9.0, temperature is 50-100° C., and time is 0.5-2.5 h.

23. The method according to claim 22, characterized in that In step (4), the aging conditions are as follows: temperature is 70-100° C., and time is 1.0-2.0 h.

24. A novel hydrocracking catalyst prepared according to any one of claims 1 to 23, characterized in that: Calculated by weight of the catalyst, the carrier content is 65% to 95%, and the content of the active metal in terms of oxide is 5% to 35%. Taking R as the radius of the catalyst particle, the silicon-aluminum material containing the Y-type molecular sieve is distributed in the range from the center to R / 2 to 2R / 3, and the aluminum oxide is distributed in the range from R / 2 to 2R / 3 to R.

25. The novel hydrocracking catalyst according to claim 24, characterized in that: The novel hydrocracking catalyst has the following properties: pore volume of 1.5 to 2.0 mL·g -1 ; Specific surface area is 300~450m 2 ·g -1 ; The pore size is ≮10nm; the particle size distribution is as follows: the proportion of particles with a diameter of less than 100μm is 0.5% to 1%, the proportion of particles with a diameter of 100 to 200μm is 2% to 5%, and the proportion of particles with a diameter of more than 200μm is 90% to 95%.

26. The novel hydrocracking catalyst according to claim 24, characterized in that: The novel hydrocracking catalyst has a pore size of 15 to 25 nm.

27. Use of the novel hydrocracking catalyst according to claim 24, 25 or 26, characterized in that: The novel hydrocracking catalyst is applied to the hydroprocessing of heavy and inferior raw materials.

Citation Information

Patent Citations

  • Waste catalyst prepares high-purity ammonium metavanadate method

    CN104628032B

  • Comprehensive utilization system of spent catalyst

    CN107723468A

  • Hydrocracking catalyst and its preparing process

    CN101468317A

  • Preparation method of hydrocracking catalyst

    CN102451744A

  • Hydrogenation catalyst as well as preparation method and application thereof

    CN104549430A