A polypropylene composite material and its preparation method and application
By adding crosslinked polyethylene and thermoplastic elastomers with specific crosslinking degrees to the polypropylene resin, the problem of insufficient flexibility and low-temperature impact resistance of polypropylene composite materials is solved, and higher impact resistance and suitable Extended range.
Patent Information
- Application Number
- CN202310433688.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-21
AI Technical Summary
The poor flexibility and insufficient low-temperature impact resistance of existing polypropylene composite materials limit their application in automobiles, home appliances and other fields.
Add crosslinked polyethylene with a specific degree of crosslinking to polypropylene resin and synergistically work with thermoplastic elastomer to improve the flexibility of the material and low-temperature impact resistance. Through the crosslinking network structure of crosslinked polyethylene and the dispersion effect of thermoplastic elastomer , enhance the impact resistance of the material.
Effectively improve the flexibility and low-temperature impact resistance of polypropylene composite materials. The impact strength of the cantilever beam notch can reach 39.8~48.6KJ/m2, the bending modulus can reach 2390~5370MPa, and the ball falling from -40℃ will not crack. It is suitable for automobiles. and preparation of household appliance materials.
Smart Images

Figure BDA0004191218620000011 
Figure BDA0004191218620000021 
Figure BDA0004191218620000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to a polypropylene composite material and a preparation method and application thereof. Background Art
[0002] Polypropylene has the advantages of low density, low price and easy processing, and has been widely used in the automotive and home appliance industries. Compared with engineering plastics, polypropylene has lower strength, and is usually reinforced by adding glass fiber or filler. However, due to the size of the glass fiber, the impact strength of the material is poor. Even if a toughening agent is added, the improvement in the impact strength of the material is limited, thus limiting its application range.
[0003] The prior art discloses a long glass fiber reinforced polypropylene composite material for 5G antenna cover and its preparation method. TPEE is selected as a toughening agent. The prepared composite material can ensure excellent impact resistance in a low temperature environment of minus 40 degrees Celsius, but this method will cause the aging performance of the material to deteriorate.
[0004] The prior art discloses a modified polypropylene material with improved impact strength, comprising polypropylene, polyolefin elastomer, high-density polyethylene, and an organic peroxide cross-linking modifier, to improve the impact strength of the polypropylene material. However, it does not make corresponding improvements on the flexibility of the polypropylene material, especially the low-temperature impact resistance of the material. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing polypropylene composite materials, namely, poor flexibility and poor low-temperature impact resistance, and to provide a polypropylene composite material. By adding cross-linked polyethylene with a specific cross-linking degree to the polypropylene resin, the synergistic effect with the thermoplastic elastomer effectively improves the flexibility and low-temperature impact resistance of the polypropylene composite material.
[0006] Another object of the present invention is to provide a method for preparing a polypropylene composite material.
[0007] Another object of the present invention is to provide an application of a polypropylene composite material in the preparation of automotive materials and household appliance materials.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A polypropylene composite material, comprising the following components by weight:
[0010]
[0011]
[0012] Wherein, the cross-linking degree of the cross-linked polyethylene is 3 to 10%, and the test method is GB / T 18474-2001;
[0013] The melt mass flow rate of the copolymerized polypropylene resin is 0.4-45 g / 10 min under the test conditions of 230°C / 2.16 kg, and the test standard is GB / T 3682.1-2018.
[0014] The present invention adds cross-linked polyethylene with a specific cross-linking degree to the polypropylene resin. Since the cross-linked polyethylene has a lower crystallinity and more amorphous regions, the polypropylene composite material can still maintain good flexibility at low temperatures. The cross-linked network structure of the cross-linked polyethylene helps to improve its entropy elasticity, can absorb more energy during impact, avoid the polypropylene composite material from rupture, and does not crack in a -40°C drop ball impact test.
[0015] With the help of thermoplastic elastomer, cross-linked polyethylene can be well dispersed in polypropylene resin, which helps to improve the impact resistance of the material. At the same time, the cross-linked network structure can avoid rupture during the energy absorption process.
[0016] The polypropylene resin of the present invention is copolymerized polypropylene. Since the copolymerized polypropylene contains ethylene segments, it has high notched impact strength and can improve compatibility with cross-linked polyethylene.
[0017] The role of glass fiber is to improve the strength of the material. The role of the compatibilizer is to improve the bonding force between glass fiber and resin, so as to further improve the strength of the material.
[0018] Preferably, the cross-linking degree of the cross-linked polyethylene is 4-6%.
[0019] Optionally, the content of the copolymerized polypropylene resin in the polypropylene composite material is not less than 30 wt.%.
[0020] Cross-linked polyethylene can be purchased from the market or prepared at home.
[0021] Preferably, the cross-linked polyethylene is mainly obtained by cross-linking reaction of polyethylene and initiator, the weight ratio of initiator to polyethylene is (0.02-0.1):100, the reaction temperature is 210-230°C, and the feeding speed is 300-500rpm.
[0022] The degree of cross-linking of cross-linked polyethylene can be controlled by the amount of initiator, reaction temperature or feeding speed.
[0023] In S1 of the present invention, polyethylene and the high-temperature initiator undergo a free radical reaction, which is relatively mild and can effectively control the degree of crosslinking of polyethylene. It can also maintain a certain flexibility while crosslinking, and can absorb impact force through deformation while avoiding the problem of rupture caused by excessive deformation.
[0024] The polyethylene may be linear low density polyethylene and / or low density polyethylene.
[0025] More preferably, the polyethylene is linear low density polyethylene.
[0026] Optionally, the melt mass flow rate of the polyethylene is 0.3-45 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 190° C. and 2.16 kg.
[0027] Preferably, the melt mass flow rate of the polyethylene is 0.5 to 30 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 190° C. and 2.16 kg.
[0028] More preferably, the melt mass flow rate of the polyethylene is 2 to 20 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 190° C. and 2.16 kg.
[0029] Preferably, the initiator is dioxane and / or polyoxane.
[0030] Optionally, the glass fiber is alkali-free glass fiber.
[0031] Preferably, the average diameter of the glass fibers is 10-14 μm.
[0032] Optionally, the melt mass flow rate of the thermoplastic elastomer is 0.4 to 22 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0033] Preferably, the melt mass flow rate of the thermoplastic elastomer is 2.1 to 20 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 230° C. and 2.16 kg.
[0034] The thermoplastic elastomer may be a polyolefin-based thermoplastic elastomer.
[0035] Optionally, the thermoplastic elastomer is ethylene propylene copolymer and / or ethylene octene copolymer (POE).
[0036] The melt mass flow rate of the thermoplastic elastomer is closer to the melt index of polypropylene, which is more conducive to promoting the dispersion of cross-linked polyethylene in polypropylene. Therefore, the compatibility of the material is improved, the impact performance is increased, and it is conducive to improving the falling ball impact effect of the material.
[0037] Preferably, the melt mass flow rate of the copolymerized polypropylene resin is 3.0-30 g / 10 min under the test conditions of 230° C. / 2.16 kg, and the test standard is GB / T 3682.1-2018.
[0038] Further preferably, the melt mass flow rate of the copolymerized polypropylene resin is 3 to 15 g / 10 min.
[0039] Preferably, the compatibilizer is one or more of maleic anhydride grafted polypropylene, maleic anhydride grafted polyethylene or maleic anhydride grafted ethylene octene copolymer.
[0040] More preferably, the compatibilizer is maleic anhydride grafted polyethylene.
[0041] Preferably, 1 to 5 parts of an antioxidant are further included, and the antioxidant includes a hindered phenol antioxidant and / or a phosphite antioxidant.
[0042] The hindered phenol antioxidant may be antioxidant 1010. The phosphite antioxidant may be antioxidant 168. The weight ratio of the hindered phenol antioxidant to the phosphite antioxidant may be 1:2.
[0043] Optionally, the weight ratio of cross-linked polyethylene to thermoplastic elastomer is 1:(0.2-0.9)
[0044] Preferably, the weight ratio of the cross-linked polyethylene to the thermoplastic elastomer is 1:(0.3-0.8).
[0045] More preferably, the weight ratio of the cross-linked polyethylene to the thermoplastic elastomer is 1:(0.5-0.7).
[0046] The invention also protects a preparation method of a polypropylene composite material, comprising the following steps: mixing the components, melting and extruding through an extruder, granulating, and drying to obtain the polypropylene composite material.
[0047] The extruder may be a twin-screw extruder.
[0048] Preferably, the method for preparing the polypropylene composite material comprises the following steps:
[0049] S1. The polyethylene, initiator and antioxidant are mixed and granulated to obtain cross-linked polyethylene;
[0050] S2. The cross-linked polyethylene, copolymerized polypropylene resin, thermoplastic elastomer, compatibilizer, antioxidant and glass fiber are mixed, melt-extruded by a twin-screw extruder, granulated, and dried to obtain the polypropylene composite material;
[0051] Among them, the weight ratio of the antioxidant in S1 to the antioxidant in S2 is (0.05-0.2):1.
[0052] The polypropylene composite material prepared by the present invention has flexibility and low-temperature impact resistance and can be widely used in the preparation of plastic products. The present invention especially protects the application of the polypropylene composite material in the preparation of automotive materials, household appliance materials and antenna cover shells.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] The polypropylene composite material of the present invention effectively improves the flexibility and low-temperature impact resistance of the polypropylene composite material by adding cross-linked polyethylene with a specific cross-linking degree into the polypropylene resin and the synergistic effect of the thermoplastic elastomer.
[0055] The polypropylene composite material of the present invention has an Izod beam notched impact strength of 39.8 to 48.6 KJ / m 2 The bending modulus can reach 2390~5370MPa, and it will not crack when subjected to falling ball impact at -40℃. DETAILED DESCRIPTION
[0056] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0057] The raw materials of each component of each embodiment of the present invention and the comparative example are shown in the following Table 1:
[0058] Table 1
[0059]
[0060]
[0061] The preparation method of cross-linked polyethylene is as follows: polyethylene, initiator, and antioxidant are added to a high-speed mixer and mixed evenly, and then added to the main feeding port of a twin-screw extruder, the extrusion temperature is controlled at 210-230°C, the feeding speed is 300-500rpm, and cross-linked polyethylene with a cross-linking degree of 3-10% is obtained by extrusion granulation.
[0062] The components and reaction conditions of the cross-linked polyethylene of the embodiments of the present invention and the comparative examples are shown in Table 2 below:
[0063] Table 2
[0064]
[0065]
[0066] Table 2
[0067]
[0068] Examples 1 to 22
[0069] A polypropylene composite material comprises the following raw material components by weight: copolymerized polypropylene resin; glass fiber; cross-linked polyethylene; thermoplastic elastomer; compatibilizer; and antioxidant.
[0070] The components of the cross-linked polyethylene are prepared as shown in Table 2.
[0071] The specific content of each component raw material is shown in Table 3 below.
[0072] Table 3 Composition of polypropylene composite materials in various embodiments (by weight)
[0073] Components 1 2 3 4 5 6 7 8 9 Cross-linked polyethylene component A1 A2 A3 A3 A3 A3 A3 A3 A3 Cross-linked polyethylene 100 100 100 49.9 200 133 123 89 84 Polypropylene resin 1 500 500 500 500 500 500 500 500 500 Glass fiber1 300 300 300 400 200 300 300 300 300 Thermoplastic elastomer 60 60 60 30 80 27 37 71 76 Compatibilizer 1 30 30 30 20 50 30 30 30 30 Antioxidant 1 1 1 1 0.5 2 1 1 1 1 Antioxidant 2 2 2 2 1.5 2.5 2 2 2 2
[0074] Table 3
[0075] Components 10 11 12 13 14 15 16 Cross-linked polyethylene component A3 A3 A3 A3 A3 A3 A3 Cross-linked polyethylene 100 100 100 100 100 100 100 Polypropylene resin 1 500 500 500 Polypropylene resin 2 500 Polypropylene resin 3 500 Polypropylene resin 5 500 Polypropylene resin 6 500 Glass fiber1 300 300 300 300 300 Fiberglass 2 300 Glass Fiber 3 300 Thermoplastic elastomer 60 60 60 60 60 60 60 Compatibilizer 1 30 30 30 30 30 30 Compatibilizer 2 30 Antioxidant 1 1 1 1 1 1 1 1 Antioxidant 2 2 2 2 2 2 2 2
[0076] The difference between Examples 17 to 22 and Example 3 is that cross-linked polyethylene components A4 to A9 are used respectively.
[0077] The preparation method of the polypropylene composite material comprises the following steps:
[0078] Add cross-linked polyethylene, copolymerized polypropylene resin, thermoplastic elastomer, compatibilizer and antioxidant into a high-speed mixer, mix well and then add into the main feeding port of a twin-screw extruder, add glass fiber into the extruder through side feeding, control the extrusion temperature at 200-230°C, control the current at 70-80%, and obtain a polypropylene composite material through extrusion granulation;
[0079] The content of components of the above polypropylene composite material was detected. In the polypropylene composite material, the contents of copolymerized polypropylene resin, glass fiber, thermoplastic elastomer, compatibilizer and antioxidant were the same as those of the raw material. The weight fractions of cross-linked polyethylene and uncross-linked polyethylene are shown in Table 4 below.
[0080] The weight fractions of the cross-linked polyethylene and the non-cross-linked polyethylene are shown in the following Table 4. ND means not detected.
[0081] Table 4
[0082]
[0083]
[0084] Comparative Examples 1 to 8
[0085] A polypropylene composite material comprises the following raw material components by weight: copolymerized polypropylene resin; glass fiber; cross-linked polyethylene; thermoplastic elastomer; compatibilizer; and antioxidant.
[0086] The components of the cross-linked polyethylene are prepared as shown in Table 2.
[0087] The specific content of each component raw material is shown in Table 5 below.
[0088] Table 5 Composition of polypropylene composite materials of each comparative example (by weight)
[0089] Components 1 2 3 4 5 6 7 8 Cross-linked polyethylene component A3 A3 0 B2 B1 A3 A3 B0 Cross-linked polyethylene 100 250 0 100 100 100 100 100 Polypropylene resin 1 500 500 500 500 500 / / 500 Polypropylene resin 7 / / / / / 500 / Polypropylene resin 4 / / / / / / 500 Glass fiber1 300 300 300 300 300 300 300 300 Thermoplastic elastomer 0 60 60 60 60 60 60 60 Compatibilizer 1 30 30 30 30 30 30 30 30 Antioxidant 1 1 1 1 1 1 1 1 1 Antioxidant 2 2 2 2 2 2 2 2 2
[0090] The preparation method of the polypropylene composite material is the same as that in the embodiment, and will not be described again here.
[0091] Results
[0092] The polypropylene composite materials of each embodiment and comparative example were tested according to the following method:
[0093] (1) Izod notched impact strength: the test standard is GB / T1843-2008; the notch type is type A.
[0094] (2) Flexural modulus: The test standard is GB / T9341-2008.
[0095] (3) Drop ball impact: The test standard is GB / T 14485-1993. The test conditions are an iron ball of 500g, heights of 1m, 1.1m and 1.2m, and a test temperature of -40°C. If the test result is no cracking, it passes; if the test result is cracking, it fails.
[0096] The specific test results of the polypropylene composite materials of each embodiment and comparative example are described in Table 6 below:
[0097] Table 6
[0098]
[0099]
[0100] It can be seen from the above data that the polypropylene composite material of the present invention has an Izod notched impact strength of 39.8 to 48.6 KJ / m 2 The bending modulus can reach 2390~5370MPa, and it will not crack when subjected to falling ball impact at -40℃.
[0101] It can be seen from Comparative Example 1 that the molecular chains of the cross-linked polyethylene are more closely connected, and the compatibility with polypropylene becomes worse. Without adding thermoplastic elastomer, a single cross-linked polyethylene cannot play a good role in improving the falling ball impact effect.
[0102] It can be seen from Comparative Example 2 that the amount of cross-linked polyethylene added is too much, and the compatibility of cross-linked polyethylene and polypropylene in the elastomer cannot be effectively improved, resulting in a decrease in the impact strength and modulus of the material, and the falling ball impact is also unqualified.
[0103] It can be seen from Comparative Example 3 that without adding cross-linked polyethylene, the pure thermoplastic elastomer has limited effect on impact enhancement and cannot improve the falling ball impact effect.
[0104] It can be seen from Comparative Example 4 that in the preparation of cross-linked polyethylene, the cross-linking degree is too large, and the compatibilizer of the cross-linked polyethylene in the polypropylene deteriorates, resulting in lower notched impact strength and worse falling ball impact.
[0105] It can be seen from Comparative Example 5 that without adding an initiator and without pre-crosslinking the polyethylene, the crosslinking degree of the crosslinked polyethylene is too low and the falling ball impact effect cannot be effectively improved.
[0106] It can be seen from Comparative Example 6 that the polypropylene resin is a homopolymer polypropylene resin, which has very poor impact strength and cannot absorb energy during the impact of a falling ball, resulting in rupture.
[0107] It can be seen from Comparative Example 7 that the melt mass flow rate of the polypropylene resin is too high and the impact performance of the material is too poor.
[0108] It can be seen from Comparative Example 8 that the cross-linking efficiency of peroxide initiators is relatively high, which easily leads to a high degree of cross-linking, thus failing the falling ball impact test.
[0109] It can be seen from Examples 1 to 3 that the amount of cross-linked polyethylene used is the same, but the content of the initiator is different, resulting in different degrees of cross-linking of the cross-linked polyethylene. The impact strength of the material first increases and then decreases. This is because as the degree of cross-linking increases, the dispersion performance in polypropylene deteriorates, resulting in a slight decrease in impact performance.
[0110] It can be seen from Examples 3 and 6 to 9 that when the degree of crosslinking of the crosslinked polyethylene is the same, when the weight ratio of the thermoplastic elastomer to the crosslinked polyethylene is (0.3 to 0.8):1, it is more conducive to the dispersion of the crosslinked polyethylene in the polypropylene, thereby improving the impact properties of the material.
[0111] It can be seen from Example 3 and Examples 10 to 13 that the polypropylene resin is copolymerized polypropylene, and the melt mass flow rate of the polypropylene resin is 3-30 g / 10 min, which is more conducive to providing certain impact strength and rigidity and meeting the material performance requirements.
[0112] It can be seen from Examples 3 and 16 that the compatibilizer is PE-g-MAH, which is more conducive to the combination of cross-linked polyethylene and glass fiber, the transmission of impact force, and the absorption of energy. Therefore, the strength and impact performance of the material are improved, which is conducive to improving the falling ball impact effect of the material.
[0113] It can be seen from Examples 3 and 17 to 19 that the melt mass flow rate of polyethylene is 2 to 20 g / 10 min, and the prepared cross-linked polyethylene can be well dispersed in the material, thus showing a good falling ball impact effect.
[0114] It can be seen from Example 3 and Example 20, Example 21 and Comparative Example 4 and Comparative Example 5 that cross-linked polyethylene with an appropriate degree of cross-linking can better increase the impact performance of the material, which is beneficial to improving the falling ball impact effect of the material.
[0115] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A polypropylene composite material, characterized in that: By weight, it includes the following components: Wherein, the cross-linking degree of the cross-linked polyethylene is 3-10%, and the test method is GB / T 18474-2001; The melt mass flow rate of the copolymerized polypropylene resin is 0.4-45g / 10min under the test conditions of 230℃ / 2.16kg, and the test standard is GB / T 3682.1-2018; The polyethylene in the cross-linked polyethylene is low-density polyethylene.
2. The polypropylene composite material according to claim 1, characterized in that: The cross-linked polyethylene is mainly obtained by cross-linking reaction of polyethylene and initiator, the weight ratio of initiator to polyethylene is (0.02-0.1):100, the reaction temperature is 210-230°C, and the rotation speed of feeding is 300-500rpm.
3. The polypropylene composite material according to claim 2, characterized in that: The melt mass flow rate of the polyethylene is 0.5 to 30 g / 10 min, the test standard is GB / T 3682.1-2018, and the test conditions are 190° C. and 2.16 kg.
4. The polypropylene composite material according to claim 2, characterized in that: The initiator is dioxane and / or polyoxane.
5. The polypropylene composite material according to claim 1, characterized in that: The average diameter of the glass fibers is 10-14 μm.
6. The polypropylene composite material according to claim 1, characterized in that: The melt mass flow rate of the thermoplastic elastomer is 2.1-20 g / 10 min, the test standard is GB / T 3682.2-2018, and the test conditions are 230° C. and 2.16 kg.
7. The polypropylene composite material according to claim 1, characterized in that: The compatibilizer is one or more of maleic anhydride grafted polypropylene, maleic anhydride grafted polyethylene or maleic anhydride grafted ethylene octene copolymer.
8. The polypropylene composite material according to claim 1, characterized in that: The invention also comprises 1 to 5 parts of an antioxidant, wherein the antioxidant comprises a hindered phenol antioxidant and / or a phosphite antioxidant.
9. The method for preparing the polypropylene composite material according to any one of claims 1 to 8, characterized in that: The steps include: The components are mixed, melt-extruded and granulated by an extruder, and dried to obtain the polypropylene composite material.
10. Use of the polypropylene composite material according to any one of claims 1 to 8 in the preparation of automotive materials, household appliance materials and antenna cover shells.
Citation Information
Cited By
A mine-used low-temperature impact-resistant polypropylene composite material and a preparation method thereof