A biodegradable material composition and preparation method thereof
The biodegradable material composition using PBST, bamboo powder, talc and other components solves the problems of high cost and insufficient performance, achieving low cost, simple process and excellent comprehensive mechanical properties. The material is completely degradable and environmentally friendly.
Patent Information
- Application Number
- CN202210012138.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-01-05
AI Technical Summary
Existing biodegradable plastics suffer from high costs and insufficient overall mechanical properties, and traditional preparation methods are not environmentally friendly.
A biodegradable material composition using components such as PBST, bamboo powder, talc, polyethylene glycol, and antioxidants is prepared by high-speed stirring and twin-screw extrusion to form a fully biodegradable material.
It achieves low cost, simple process and excellent comprehensive mechanical properties, and the material is completely biodegradable and environmentally friendly.
Smart Images

Figure BDA0003456902640000031
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer materials, and in particular, relates to a biodegradable material composition and a method for preparing the biodegradable material composition. Background Art
[0002] Traditional plastic materials, such as polypropylene (PP), polyethylene (PE), polystyrene (PS), polyethylene terephthalate (PET), polyvinyl chloride (PVC), etc., have excellent properties, can meet human needs in all aspects, and bring great convenience to human life. But at the same time, these plastics are difficult to degrade under natural conditions. With the increasing use, a large amount of plastics are scattered in nature, becoming "white pollution" that is difficult to deal with, bringing more and more problems to the environment and ecology. At present, with the continuous improvement of environmental protection standards, it has become a trend to use more environmentally friendly biodegradable plastics to replace traditional non-degradable plastics. Common biodegradable plastics on the market include polybutylene terephthalate-adipate-butylene ester (PBAT), polybutylene succinate and polycaprolactone (PCL). However, there are currently two factors that restrict the large-scale promotion of the above-mentioned biodegradable plastics. One is that the price of synthetic biodegradable plastics is generally expensive, and the other is that the comprehensive mechanical properties of many biodegradable materials cannot meet the requirements of actual use.
[0003] In order to solve the above two problems, a commonly used method is to prepare multi-component materials. That is, other components are introduced into biodegradable plastic materials to achieve the purpose of reducing costs or improving performance. However, some issues still need to be paid attention to in this process, such as the degradability and environmental friendliness of the introduced components. If the introduced components are non-degradable plastics, the impact of the resulting materials on the environment may be even worse; the environmental friendliness of the preparation process must also be considered. For example, patent document CN104672825A discloses a PBAT / nanocellulose degradable composite material and a preparation method thereof. The method uses chloroform as a solution to blend nanocellulose with PBAT. A large amount of organic solvents are required in this method, which is not friendly to the environment. For example, patent document CN112608585A discloses a biodegradable composite material composed of PLA, PBAT, montmorillonite, ester exchange catalyst, toughening agent and lubricant. Two kinds of plastics are used, which increases the cost and process complexity. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the purpose of the present invention is to provide a biodegradable material composition and a preparation method thereof and a film product. Each component in the composition is a completely biodegradable material. At the same time, the composition has excellent comprehensive mechanical properties. More importantly, the composition is low in cost and simple in processing method.
[0005] The first aspect of the present invention provides a biodegradable material composition, which is composed of the following raw materials: PBST, bamboo powder, talcum powder, polyethylene glycol, optionally a chain extender and optionally an antioxidant;
[0006] Based on the total weight of PBST, bamboo powder and talcum powder, the amount of PBST is 65-95% by weight, the amount of bamboo powder is 3-20% by weight, and the amount of talcum powder is 1-15% by weight; the amount of polyethylene glycol is 2-20% of the total weight of PBST, bamboo powder and talcum powder, the amount of chain extender is 0-5% of the total weight of PBST, bamboo powder and talcum powder, and the amount of antioxidant is 0-1.5% of the total weight of PBST, bamboo powder and talcum powder.
[0007] The second aspect of the present invention provides a method for preparing the above-mentioned biodegradable material composition, which comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.
[0008] The composition of the invention is completely biodegradable, has a simple and easy preparation method, low cost and good comprehensive performance.
[0009] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0010] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0011] According to a first aspect of the present invention, the present invention provides a biodegradable material composition, which is composed of the following raw materials: PBST, bamboo powder, talcum powder, polyethylene glycol, optionally a chain extender and optionally an antioxidant;
[0012] Based on the total weight of PBST, bamboo powder and talcum powder, the amount of PBST is 65-95% by weight, the amount of bamboo powder is 3-20% by weight, and the amount of talcum powder is 1-15% by weight; the amount of polyethylene glycol is 2-20% of the total weight of PBST, bamboo powder and talcum powder, the amount of chain extender is 0-5% of the total weight of PBST, bamboo powder and talcum powder, and the amount of antioxidant is 0-1.5% of the total weight of PBST, bamboo powder and talcum powder.
[0013] In the present invention, the PBST (polybutylene terephthalate-polybutylene succinate copolymer) is a copolymer containing repeating units represented by formula (I) and (II);
[0014]
[0015] In formula (I), m1=4, n1=2;
[0016] In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol %.
[0017] In the present invention, the particle size of the bamboo powder is 50-200 meshes.
[0018] According to the present invention, the particle size of the talc is 325-8000 mesh.
[0019] In the present invention, the molecular weight of the polyethylene glycol is 200-600 g / mol.
[0020] Preferably, based on the total weight of PBST, bamboo powder and talcum powder, the amount of PBST is 75-95% by weight, the amount of bamboo powder is 3-15% by weight, and the amount of talcum powder is 1-10% by weight.
[0021] According to the present invention, the chain extender and antioxidant may be various types conventionally used in the prior art. For example, the antioxidant may be a hindered phenol antioxidant, a phosphite antioxidant, or a pentaerythritol ester antioxidant; the chain extender may be a difunctional acid derivative, an isocyanate, an anhydride, or an epoxide.
[0022] In the present invention, various raw materials can be prepared or commercially available, and the present invention has no particular limitation on their sources, as long as the above-mentioned parameter requirements are met.
[0023] The PBST in the present invention can be prepared by the following method, which specifically comprises the following steps:
[0024] (1) contacting and prepolymerizing a diacid, an ester thereof, an anhydride thereof or a mixture thereof, a diol, and a first catalyst in a reaction vessel under vacuum conditions to obtain a prepolymer; the diacid refers to an organic dicarboxylic acid, such as terephthalic acid and succinic acid; and the diol refers to a primary diol, including butanediol;
[0025] (2) A second catalyst is brought into contact with the prepolymer to perform a vacuum polycondensation reaction to obtain the PBST (polybutylene terephthalate-polybutylene succinate copolymer).
[0026] The present invention has no particular limitation on the mixing order of the components in the reaction system, and the amount of each component used is based on the content of the structural units required by the product.
[0027] According to the present invention, the reaction conditions of each step may also adopt conventional conditions in the art.
[0028] Specifically, in step (1), the reaction conditions of the prepolymerization may include: reaction temperature of 190-250° C.; vacuum degree of 200-600 Pa; reaction time of 1-3 hours, or until the small molecules in the reaction system are almost exhausted and the fraction temperature remains unchanged.
[0029] In step (2), the reaction conditions of the vacuum polycondensation reaction may include: reaction temperature of 200-300° C.; vacuum degree of <300 Pa; and reaction time of 3-12 hours.
[0030] The present invention does not particularly limit the catalyst used in the polymerization reaction and its amount, and can be various conventional catalysts and conventional catalyst amounts for synthesizing polyester. The catalysts used in step (1) and step (2) can be the same or different. For example, the catalyst used in step (1) can be selected from at least one of compounds of metal titanium, antimony and tin; the catalyst used in step (2) can be selected from compounds of rare earth metal Ln and mixtures thereof, wherein the rare earth metal Ln is selected from at least one of lanthanide elements, scandium and yttrium.
[0031] According to the present invention, step (1) and step (2) can be carried out in the same reactor or in different reactors, that is, the prepolymer can be taken out and transferred to another reactor to continue the subsequent polymerization reaction.
[0032] According to the present invention, nitrogen is usually used as protection in the reaction system, but other atmospheres, including air, may also be used.
[0033] According to the second aspect of the present invention, the present invention provides a method for preparing the above-mentioned biodegradable material composition, which comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.
[0034] In the present invention, the mixing time is 1-10 minutes.
[0035] According to the present invention, the setting temperature of the twin-screw extruder is 110-130°C.
[0036] The substances and parameters not limited in the present invention can be selected according to the existing technology and belong to the conventional technical means in this field.
[0037] The present invention will be further described below with reference to the following examples, but is not limited to these examples.
[0038] In the following examples and comparative examples, the relevant data were obtained according to the following test methods:
[0039] 1. The crystallization temperature of the material is measured by TA's Q-100 DSC. The sample is first isothermally heated at 200°C for 5 minutes to eliminate the thermal history, and then cooled at 10°C / min. The crystallization temperature is calculated according to the peak temperature of the crystallization peak.
[0040] 2. The tensile strength of the material is measured in accordance with GB / T 1040.
[0041] Examples 1-12 are provided to illustrate the compositions and methods of making the same of the present invention.
[0042] Example 1
[0043] Polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder, and talcum powder are mixed in a weight ratio of 80:15:5, and then 0.1% by weight of a chain extender, 5% by weight of polyethylene glycol, and 0.3% by weight of an antioxidant are added to the above materials. The weight fractions of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST, bamboo powder, and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Bamboo powder is commercially available, 200 mesh, and talcum powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company. ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0044] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixed material; the mixed material was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C. After extrusion and pelletization, the biodegradable material composition was obtained.
[0045] Example 2
[0046] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 45%.
[0047] Example 3
[0048] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 55%.
[0049] Example 4
[0050] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder and talcum powder are prepared in a weight ratio of 75:20:5.
[0051] Example 5
[0052] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder and talc are prepared in a weight ratio of 84:15:1.
[0053] Example 6
[0054] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder and talcum powder are prepared in a weight ratio of 94:5:1.
[0055] Example 7
[0056] Same as Example 1, except that the particle size of the bamboo powder is changed to 50 mesh.
[0057] Example 8
[0058] Same as Example 1, except that the particle size of talc is changed to 325 mesh.
[0059] Example 9
[0060] Same as Example 1, except that the particle size of talc powder is changed to 8000 mesh.
[0061] Example 10
[0062] Same as Example 1, except that the weight fraction of polyethylene glycol is changed to 20%.
[0063] Embodiment 11
[0064] Same as Example 1, except that the weight fraction of polyethylene glycol is changed to 2%.
[0065] Example 12
[0066] Same as Example 1, except that the molecular weight of polyethylene glycol is changed to 200 g / mol.
[0067] Comparative Example 1
[0068] Take polybutylene terephthalate-polybutylene succinate copolymer (PBST) material, add 0.1 wt% chain extender and 0.3 wt% antioxidant to the material. The weight fractions of the chain extender and antioxidant are calculated according to the weight of PBST. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. The chain extender is BASF's ADR 4468. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0069] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixture; the mixture was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C., and after extrusion and pelletization, a composite material was obtained.
[0070] Comparative Example 2
[0071] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are mixed in a weight ratio of 95:5, and then 0.1 weight% of chain extender, 5 weight% of polyethylene glycol, and 0.3 weight% of antioxidant are added to the above materials. The weight fractions of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Research Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company. ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0072] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixture; the mixture was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C., and after extrusion and pelletization, a composite material was obtained.
[0073] Comparative Example 3
[0074] Polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder, and talcum powder are mixed in a weight ratio of 80:15:5, and then 0.1% by weight of a chain extender and 0.3% by weight of an antioxidant are added to the above materials. The weight fractions of the above chain extender and antioxidant are calculated based on the sum of the weights of PBST, bamboo powder, and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Bamboo powder is commercially available, 200 mesh, and talcum powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company. ADR 4468. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0075] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixed material; the mixed material was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C. After extrusion and pelletization, the biodegradable material composition was obtained.
[0076] Comparative Example 4
[0077] Polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder, and talcum powder are mixed in a weight ratio of 65:30:5, and then 0.1% by weight of a chain extender, 5% by weight of polyethylene glycol, and 0.3% by weight of an antioxidant are added to the above materials. The weight fractions of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST, bamboo powder, and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Bamboo powder is commercially available, 200 mesh, and talcum powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company. ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0078] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixed material; the mixed material was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C. After extrusion and pelletization, the biodegradable material composition was obtained.
[0079] Comparative Example 5
[0080] Polybutylene terephthalate-polybutylene succinate copolymer (PBST), bamboo powder, and talcum powder are mixed in a weight ratio of 94:1:5, and then 0.1% by weight of a chain extender, 5% by weight of polyethylene glycol, and 0.3% by weight of an antioxidant are added to the above materials. The weight fractions of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST, bamboo powder, and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Bamboo powder is commercially available, 200 mesh, and talcum powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company. ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1.
[0081] The raw materials were added into a high-speed mixer for mixing for 5 minutes to obtain a mixed material; the mixed material was added into a twin-screw extruder for melting, the set temperature of the twin-screw extruder was 130° C. After extrusion and pelletization, the biodegradable material composition was obtained.
[0082] The compositions obtained in the examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.
[0083] Table 1
[0084] Tensile modulus / MPa Elongation at break / % Crystallization temperature / ℃ Example 1 137.8 95 103.2 Example 2 111.2 102 96.7 Example 3 162.7 70 115.4 Example 4 182.3 63 102.8 Example 5 116.2 102 102.5 Example 6 103.7 179 102.1 Example 7 133.3 80 103.3 Example 8 129.6 81 103.2 Example 9 142.7 92 103.8 Example 10 136.4 94 103.1 Embodiment 11 119.3 83 103.5 Example 12 116.2 88 103.3 Comparative Example 1 55.8 341 78.3 Comparative Example 2 69.7 210 104.5 Comparative Example 3 133.2 33 103.1 Comparative Example 4 221.7 9 103.3 Comparative Example 5 70.2 317 103.6
[0085] As can be seen from Table 1, compared with Comparative Example 1, i.e., when bamboo powder, talcum powder and polyethylene glycol are not added, Example 1 adds bamboo powder, talcum powder and polyethylene glycol, and its modulus and crystallization temperature are significantly improved, while a high elongation at break can be maintained. Referring to Comparative Example 3, under the same conditions, if polyethylene glycol is not added, the elongation at break will decrease significantly. Examples 2 and 3 also have good comprehensive properties when changing the PBST copolymer composition. Examples 4-12 give the effects of changing the composition, bamboo powder and talcum powder particle size, and polyethylene glycol molecular weight, etc., and the materials under the above conditions have a good combination of rigidity and toughness. Compared with Comparative Example 2, it can be seen that without adding bamboo powder, the rigidity cannot reach a higher level. It can be seen from Comparative Example 1 that without adding talcum powder, the crystallization temperature cannot reach a higher level. Comparative Example 4 shows that when the bamboo powder content is too high, although the rigidity is very high, the elongation at break is too low, and the comprehensive properties of such materials cannot meet the requirements. It can be seen from comparative example 5 that when the bamboo powder content is low, the rigidity cannot reach a good level. In summary, within the range required by the present invention, a good rigidity-toughness balance and crystallinity are achieved, and the material has good comprehensive performance.
[0086] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A biodegradable material composition, characterized in that: The composition is composed of the following raw materials: PBST, bamboo powder, talcum powder, polyethylene glycol, chain extender and antioxidant; Based on the total weight of PBST, bamboo powder and talc, the amount of PBST is 65-95% by weight, the amount of bamboo powder is 3-20% by weight, and the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-20% of the total weight of PBST, bamboo powder and talc, the amount of chain extender is 0.1-5% of the total weight of PBST, bamboo powder and talc, and the amount of antioxidant is 0.3-1.5% of the total weight of PBST, bamboo powder and talc; The PBST is a copolymer containing repeating units represented by formula (I) and (II); Formula (I) Formula (II) In formula (I), m1=4, n1=2; In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol%; The particle size of the bamboo powder is 50-200 mesh; The particle size of the talcum powder is 325-8000 mesh; The molecular weight of the polyethylene glycol is 200-600 g / mol.
2. The biodegradable material composition according to claim 1, wherein: Based on the total weight of PBST, bamboo powder and talcum powder, the amount of PBST is 75-95% by weight, the amount of bamboo powder is 3-15% by weight, and the amount of talcum powder is 1-10% by weight.
3. The method for preparing the biodegradable material composition according to claim 1 or 2, characterized in that: The preparation method comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.
4. The method for preparing the biodegradable material composition according to claim 3, wherein: The mixing time is 1-10 min.
5. The method for preparing the biodegradable material composition according to claim 3, wherein: The setting temperature of the twin-screw extruder is 110-130°C.