A biodegradable material composition and its preparation method and film product

By using compositions of materials such as PBST, talc, polyethylene glycol, etc., the problems of low production efficiency and uneven thickness in film processing are solved, and high-quality and low-cost biodegradable film products are achieved to meet the rapid production and high-quality control needs.

CN116444956BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210012139.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-05
Publication Date
2024-11-19
Estimated Expiration
2042-01-05

AI Technical Summary

Technical Problem

In film processing, existing biodegradable materials have low production efficiency, uneven product thickness, and easy bonding in blow molding process, making it difficult to meet the needs of rapid production and high-quality control.

Method used

Using a biodegradable material composition composed of PBST, talc, polyethylene glycol, chain extender and antioxidant, the film products suitable for a variety of blow molding processes are prepared by high-speed stirring and twin-screw extruder processing. , improve production speed and film stability.

Benefits of technology

It realizes rapid and stable production of film products, uniform thickness, not easy to bond, excellent comprehensive performance, low cost, stable film bubbles and no wrinkles during processing, significantly improving mechanical strength and processing rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003456905400000031
    Figure BDA0003456905400000031
  • Figure BDA0003456905400000102
    Figure BDA0003456905400000102
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer materials, and discloses a biodegradable material composition, a preparation method thereof and a film product, wherein the composition is composed of the following raw materials: PBST, talcum powder, polyethylene glycol, optionally a chain extender and optionally an antioxidant; based on the total weight of PBST and talcum powder, the amount of PBST is 85-99% by weight, and the amount of talcum powder is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talcum powder, the amount of the chain extender is 0-5% of the total weight of PBST and talcum powder, and the amount of the antioxidant is 0-1.5% of the total weight of PBST and talcum powder. The film product prepared by the composition has stable size, is not easy to bond, has uniform thickness, has good comprehensive performance, and has a fast production speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer materials, and in particular, relates to a biodegradable material composition, a preparation method of the biodegradable material composition, and a film product made from the biodegradable material composition. Background Art

[0002] With the continuous improvement of environmental protection standards, it has become a trend to use more environmentally friendly biodegradable plastics to replace traditional non-degradable plastics, especially in the field of films, such as express packaging films, supermarket shopping bags and other application fields, biodegradable materials have very broad development prospects. Common process types in film processing include calendering, blow molding, cast film and stretching. The blown film process has strong raw material adaptability and is one of the most common processing methods used in all films. In the blown film process, speeding up the production line speed and optimizing the uniformity of film thickness are of great significance in production efficiency and product quality control. Summary of the invention

[0003] In order to improve production efficiency and product quality, the purpose of the present invention is to provide a biodegradable material composition, a preparation method thereof and a film product. The composition is suitable for rapid production and is applicable to various blow molding processes such as flat blowing, upward blowing and downward blowing. The blow molding production line of the film product is fast, and the film product has stable dimensions, is not easy to stick together, has uniform thickness and has good comprehensive performance.

[0004] The first aspect of the present invention provides a biodegradable material composition, which is composed of the following raw materials: PBST, talc, polyethylene glycol, optionally a chain extender and optionally an antioxidant;

[0005] Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0-5% of the total weight of PBST and talc, and the amount of antioxidant is 0-1.5% of the total weight of PBST and talc.

[0006] The second aspect of the present invention provides a method for preparing the above-mentioned biodegradable material composition, which comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.

[0007] The third aspect of the present invention provides a biodegradable film product, which is prepared using the above composition.

[0008] The film product prepared by using the composition of the present invention has good comprehensive mechanical properties, the preparation method of the film product is simple, the cost is low, the film bubble is stable during the processing, the film thickness is uniform, there is no wrinkle, and it does not stick and close, and rapid and stable production can be achieved.

[0009] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0010] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0011] According to a first aspect of the present invention, the present invention provides a biodegradable material composition, which is composed of the following raw materials: PBST, talc, polyethylene glycol, optionally a chain extender and optionally an antioxidant;

[0012] Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0-5% of the total weight of PBST and talc, and the amount of antioxidant is 0-1.5% of the total weight of PBST and talc.

[0013] In the present invention, the PBST (polybutylene terephthalate-polybutylene succinate copolymer) is a copolymer containing repeating units represented by formula (I) and (II);

[0014]

[0015] In formula (I), m1=4, n1=2;

[0016] In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol %.

[0017] According to the present invention, the particle size of the talc powder is 325-8000 mesh, preferably 2000-8000 mesh.

[0018] In the present invention, the molecular weight of the polyethylene glycol is 200-600 g / mol.

[0019] Preferably, based on the total weight of PBST and talc, the amount of PBST is 90-99 weight %, and the amount of talc is 1-10 weight %.

[0020] According to the present invention, the chain extender and antioxidant may be various types conventionally used in the prior art. For example, the antioxidant may be a hindered phenol antioxidant, a phosphite antioxidant, or a pentaerythritol ester antioxidant; the chain extender may be a difunctional acid derivative, an isocyanate, an anhydride, or an epoxide.

[0021] In the present invention, various raw materials can be prepared or commercially available, and the present invention has no particular limitation on their sources, as long as the above-mentioned parameter requirements are met.

[0022] The PBST in the present invention can be prepared by the following method, which specifically comprises the following steps:

[0023] (1) contacting and prepolymerizing a diacid, an ester thereof, an anhydride thereof or a mixture thereof, a diol, and a first catalyst in a reaction vessel under vacuum conditions to obtain a prepolymer; the diacid refers to an organic dicarboxylic acid, such as terephthalic acid and succinic acid; and the diol refers to a primary diol, including butanediol;

[0024] (2) A second catalyst is brought into contact with the prepolymer to perform a vacuum polycondensation reaction to obtain the PBST (polybutylene terephthalate-polybutylene succinate copolymer).

[0025] The present invention has no particular limitation on the mixing order of the components in the reaction system, and the amount of each component used is based on the content of the structural units required by the product.

[0026] According to the present invention, the reaction conditions of each step may also adopt conventional conditions in the art.

[0027] Specifically, in step (1), the reaction conditions of the prepolymerization may include: reaction temperature of 190-250° C.; vacuum degree of 200-600 Pa; reaction time of 1-3 hours, or until the small molecules in the reaction system are almost exhausted and the fraction temperature remains unchanged.

[0028] In step (2), the reaction conditions of the vacuum polycondensation reaction may include: reaction temperature of 200-300° C.; vacuum degree of <300 Pa; and reaction time of 3-12 hours.

[0029] The present invention does not particularly limit the catalyst used in the polymerization reaction and its amount, and can be various conventional catalysts and conventional catalyst amounts for synthesizing polyester. The catalysts used in step (1) and step (2) can be the same or different. For example, the catalyst used in step (1) can be selected from at least one of compounds of metal titanium, antimony and tin; the catalyst used in step (2) can be selected from compounds of rare earth metal Ln and mixtures thereof, wherein the rare earth metal Ln is selected from at least one of lanthanide elements, scandium and yttrium.

[0030] According to the present invention, step (1) and step (2) can be carried out in the same reactor or in different reactors, that is, the prepolymer can be taken out and transferred to another reactor to continue the subsequent polymerization reaction.

[0031] According to the present invention, nitrogen is usually used as protection in the reaction system, but other atmospheres, including air, may also be used.

[0032] According to the second aspect of the present invention, the present invention provides a method for preparing the above-mentioned biodegradable material composition, which comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.

[0033] In the present invention, the mixing time may be 1-10 min.

[0034] The third aspect of the present invention provides a biodegradable film product, which is prepared using the above composition.

[0035] According to the present invention, the film product is obtained by blow molding.

[0036] The blow molding method used in the present invention can be conventionally configured according to the prior art, and the following main configurations and conditions are applicable:

[0037] 1) The screw length can be 20 to 40 times the screw diameter.

[0038] 2) The barrel and mold temperature can be between 110-180℃.

[0039] 3) The blow-up ratio can be 2 to 4.

[0040] 4) The die diameter can be any commercial die size.

[0041] 5) Film cooling can be performed with a cooling fluid, which can be liquid or gaseous. In the case of cooling with a liquid cooling medium, water is the preferred cooling medium, and the extrusion direction can be vertically downward. In the case of cooling with a gaseous cooling medium, air is the preferred cooling medium, but other gases, such as nitrogen, can also be used, and the extrusion direction is preferably vertically upward.

[0042] 6) The cooling medium temperature can be 5 to 20°C.

[0043] 7) The extrusion and blowing device is a film blowing device well known in the art.

[0044] The substances and parameters not limited in the present invention can be selected according to the existing technology and belong to the conventional technical means in this field.

[0045] The present invention will be further described below with reference to the following examples, but is not limited to these examples.

[0046] In the following examples and comparative examples, the relevant data were obtained according to the following test methods:

[0047] 1. Mechanical properties test: All mechanical properties were tested by Instron 5965 universal testing machine.

[0048] 2. The crystallization temperature of the material is measured by TA's Q-100 DSC. The sample is first isothermally heated at 200°C for 5 minutes to eliminate the thermal history, and then cooled at 10°C / min. The crystallization temperature is calculated according to the peak temperature of the crystallization peak.

[0049] Examples 1-13 are provided to illustrate the compositions and methods of making the same of the present invention.

[0050] Example 1

[0051] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1 weight % of chain extender, 5 weight % of polyethylene glycol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer for 5 minutes, and the resulting mixture is melted in a twin-screw extruder, extruded and pelletized to obtain a composite.

[0052] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0053] Example 2

[0054] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 95:5.

[0055] Example 3

[0056] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 90:10.

[0057] Example 4

[0058] Same as Example 1, except that polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talc are prepared in a weight ratio of 85:15.

[0059] Example 5

[0060] Same as Example 1, except that the particle size of talc is changed to 8000 mesh.

[0061] Example 6

[0062] Same as Example 1, except that the particle size of talc is changed to 2000 mesh.

[0063] Example 7

[0064] Same as Example 1, except that the particle size of talc is changed to 325 mesh.

[0065] Example 8

[0066] Same as Example 1, except that the weight fraction of polyethylene glycol is adjusted to 15%.

[0067] Example 9

[0068] Same as Example 1, except that the weight fraction of polyethylene glycol is adjusted to 2%.

[0069] Example 10

[0070] Same as Example 1, except that the molecular weight of polyethylene glycol is changed to 200 g / mol.

[0071] Embodiment 11

[0072] Same as Example 1, except that the molecular weight of polyethylene glycol is changed to 400 g / mol.

[0073] Example 12

[0074] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 45%.

[0075] Example 13

[0076] Same as Example 1, except that the molar content of the repeating unit (II) in the polybutylene terephthalate-polybutylene succinate copolymer (PBST) is 55%.

[0077] Comparative Example 1

[0078] Take polybutylene terephthalate-polybutylene succinate copolymer (PBST) material, add 0.1 wt% chain extender and 0.3 wt% antioxidant to the material. The weight percentages of the chain extender and antioxidant are calculated based on the weight of PBST. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. The chain extender is BASF's ADR4468. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials were first mixed in a high-speed mixer for 5 minutes, and the obtained mixture was melted in a twin-screw extruder, and extruded and pelletized to obtain a composite.

[0079] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0080] Comparative Example 2

[0081] Take polybutylene terephthalate-polybutylene succinate copolymer (PBST), add 0.1 wt% of chain extender, 5 wt% of polyethylene glycol, and 0.3 wt% of antioxidant to the above material. The weight percentages of the above chain extender, polyethylene glycol, and antioxidant are all calculated according to the weight of PBST. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. The chain extender is BASF's ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer for 5 minutes, and the resulting mixture is melted in a twin-screw extruder, extruded and pelletized to obtain a composite.

[0082] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0083] Comparative Example 3

[0084] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1% by weight of a chain extender and 0.3% by weight of an antioxidant are added to the above materials. The weight percentages of the above chain extender and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc powder comes from Maclean Company, 5000 mesh. The chain extender is from BASF Company ADR4468. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials were first mixed in a high-speed mixer for 5 minutes, and the obtained mixture was melted in a twin-screw extruder, and extruded and pelletized to obtain a composite.

[0085] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0086] Comparative Example 4

[0087] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 80:20, and then 0.1 weight % of chain extender, 5 weight % of polyethylene glycol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, polyethylene glycol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Institute of Chemical Industry, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Polyethylene glycol comes from Shanghai Aladdin Biochemical Technology Co., Ltd., with a molecular weight of 600 g / mol. The antioxidant is prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials are first mixed in a high-speed mixer for 5 minutes, and the resulting mixture is melted in a twin-screw extruder, extruded and pelletized to obtain a composite.

[0088] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0089] Comparative Example 5

[0090] Polybutylene terephthalate-polybutylene succinate copolymer (PBST) and talcum powder are prepared in a weight ratio of 99:1, and then 0.1 weight % of chain extender, 5 weight % of glycerol, and 0.3 weight % of antioxidant are added to the above materials. The weight percentages of the above chain extender, glycerol, and antioxidant are calculated based on the sum of the weights of PBST and talcum powder. Among them, polybutylene terephthalate-polybutylene succinate copolymer (PBST) is a pilot product of Beijing Chemical Research Institute, and the molar content of repeating unit (II) is 50%. Talc comes from McLean Company, 5000 mesh. The chain extender is from BASF Company ADR 4468. Glycerol was obtained from Shanghai Aladdin Biochemical Technology Co., Ltd. The antioxidant was prepared by mixing BASF1010 and BASF168 in a weight ratio of 1:1. The raw materials were first mixed in a high-speed mixer for 5 minutes, and the obtained mixture was melted in a twin-screw extruder, and extruded and pelletized to obtain a composite.

[0091] The obtained composition was processed into a film product by blow molding. The specific production conditions and film properties are shown in Table 1.

[0092] Table 1

[0093]

[0094] Note: MD stands for machine direction and TD stands for transverse direction.

[0095] As can be seen from Table 1, the addition of talcum powder in the composition of the present invention can increase the crystallization temperature of PBST by more than 20°C, so the crystallization solidification rate of the melt can be significantly increased, the production speed can be accelerated, and the film stability can be improved at the same time, and the problems such as collapse and wrinkles are not easy to occur, and adhesion is avoided. In addition, the addition of talcum powder can also improve the mechanical strength of PBST film products and significantly improve the processing rate. There is a range for the content and particle size of talcum powder, within which rapid processing and film stability can be met, and the resulting film has a good balance of rigidity and toughness. Beyond this range, it does not have the above characteristics. The function of polyethylene glycol is to significantly increase the elongation at break of the material, so that the film has good toughness and is not easy to break. It can be seen that within the required composition range, the material has a good balance of rigidity and toughness.

[0096] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A biodegradable material composition, characterized in that: The composition is composed of the following raw materials: PBST, talcum powder, polyethylene glycol, chain extender and antioxidant; Based on the total weight of PBST and talc, the amount of PBST is 85-99% by weight, and the amount of talc is 1-15% by weight; the amount of polyethylene glycol is 2-15% of the total weight of PBST and talc, the amount of chain extender is 0.1-5% of the total weight of PBST and talc, and the amount of antioxidant is 0.3-1.5% of the total weight of PBST and talc; The PBST is a copolymer containing repeating units represented by formula (I) and (II); Formula (I) Formula (II) In formula (I), m1=4, n1=2; In the PBST, the content of the repeating unit represented by formula (II) is 45-55 mol%; The particle size of the talcum powder is 325-8000 mesh; The molecular weight of the polyethylene glycol is 200-600 g / mol.

2. The biodegradable material composition according to claim 1, wherein: The particle size of the talcum powder is 2000-8000 mesh.

3. The biodegradable material composition according to claim 1, wherein: Based on the total weight of PBST and talc, the amount of PBST used is 90-99 weight %, and the amount of talc used is 1-10 weight %.

4. The method for preparing the biodegradable material composition according to any one of claims 1 to 3, characterized in that: The preparation method comprises: adding various raw materials into a high-speed mixer for mixing to obtain a mixed material; adding the mixed material into a twin-screw extruder for melting, and obtaining the biodegradable material composition after extrusion and pelletizing.

5. The method for preparing the biodegradable material composition according to claim 4, wherein: The mixing time is 1-10 min.

6. A biodegradable film product, characterized in that: The film product is prepared by using the composition described in any one of claims 1 to 3.

7. The biodegradable film product according to claim 6, wherein: The film product is obtained by adopting a blow molding method.