A kind of weather-resistant and alkali-resistant anticorrosive coating and preparation method thereof
Through the design of two-dimensional nano-modified solvent-free epoxy internal drag-reducing coating, the problem of poor performance of existing coatings in high concentration alkali environments is solved, and the protection performance of weathering and alkali resistance and construction convenience is achieved. For long-term outdoor use.
Patent Information
- Application Number
- CN202310451703.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-25
AI Technical Summary
The existing weather-resistant, acid-resistant and alkali-resistant coatings have poor performance when used in high-concentration alkali environments, high costs and harsh construction conditions, making it difficult to use outdoors for a long time.
Two-dimensional nanomodified solvent-free epoxy internal drag-reducing coating is composed of chloroether resin, xylene, polymer carboxylic acid, modified polysiloxane, polyamide wax, pigment, drying agent and butyl acetate. The paint component and the curing agent component of hexamethylene diisocyanate are prepared, and a weather-resistant and alkali-resistant anticorrosion coating is adopted. It adopts a simple spraying method and has good anticorrosion, wear resistance, drag reduction and shielding protection performance.
The paint is soaked in a 35% alkali liquid environment for 10,000 hours at room temperature for 10,000 hours, the paint film is intact, low cost, convenient construction, and suitable for long-term outdoor use.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a weather-resistant and alkali-resistant anticorrosive coating and a preparation method thereof. Background Art
[0002] At present, weather-resistant, acid-resistant, and alkali-resistant coatings are generally single in nature. It is difficult to produce coatings that provide long-term protection in an environment that requires alkali resistance and weather resistance with current technology. Even coatings produced using alternative technologies based on environmental requirements have very high costs.
[0003] In terms of paint film quality, the existing technology uses acrylic resin to improve weather resistance, and epoxy resin and plasticizer to improve adhesion and basic physical properties. Conventional thermoplastic acrylic resin, epoxy resin and plasticizer cannot be used for a long time in a high-concentration alkaline environment, and can only be protected for a short time in an alkaline environment with a concentration of less than 3%. In addition, epoxy resin and plasticizer have poor weather resistance and cannot be used in outdoor environments for a long time. Chinese patents CN105838192A and CN102277083A use epoxy polysiloxane coatings, but they are expensive and cannot be used in concentrated alkaline environments for a long time. They are also demanding on construction conditions and require moisture curing reactions to form protective coatings, which is inconvenient for construction.
[0004] Therefore, it is of great significance to provide a coating with super weather resistance and alkali resistance. Summary of the invention
[0005] The invention provides a two-dimensional nano-modified solvent-free epoxy internal drag-reducing coating and a preparation method thereof. The coating has good corrosion resistance, wear resistance and drag-reducing properties and also has good shielding protection performance.
[0006] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 33-50% of a paint component and 50-67% of a curing agent component;
[0007] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0008] Chloroether resin 10-30%, xylene 20-40%, mixture of polymer carboxylic acid and modified polysiloxane 0.2-3%, polyamide wax 0.3-1%, pigment 15-40%, drying agent 0.1-1%, butyl acetate 8-20%.
[0009] Preferably, the curing agent component is hexamethylene diisocyanate.
[0010] Preferably, the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:(1-3).
[0011] Preferably, the paint component is composed of the following raw materials in terms of weight percentage: 13-28% chloroether resin, 25-38% xylene, 0.2-1.3% mixture of polymer carboxylic acid and modified polysiloxane, 0.3-1% polyamide wax, 22-40% pigment, 0.5-1% drying agent, and 11-15% butyl acetate.
[0012] Preferably, the paint component is composed of the following raw materials in weight percentage: 18-25% chloroether resin, 27-35% xylene, 0.5-1.3% mixture of polymer carboxylic acid and modified polysiloxane, 0.3-0.8% polyamide wax, 22-37% pigment, 0.6-1% drying agent, and 12-15% butyl acetate.
[0013] Preferably, the drier is an organotin drier.
[0014] Preferably, the drier is T-12 organotin drier.
[0015] Preferably, the pigment is red iron oxide.
[0016] The preparation method of the weather-resistant and alkali-resistant anticorrosive coating comprises the following steps:
[0017] (1) Add chloroether resin, xylene, a mixture of high molecular weight carboxylic acid and modified polysiloxane, and polyamide wax while stirring and mixing. After the mixing is completed, continue stirring for 10-30 minutes, grind, and then add pigment, drying agent, and butyl acetate, and stir and mix;
[0018] (2) Add the curing agent component to the product of step (1) and stir to mix.
[0019] Preferably, the grinding is performed by using a horizontal sand mill to grind to a fineness of less than 30 nm.
[0020] Advantages of the present invention:
[0021] The coating provided by the present invention has a simple preparation method and low cost, can be constructed under conventional conditions, can be directly sprayed, has good weather resistance and alkali resistance, can be used in an alkaline environment for a long time, and can be immersed in a 35% alkali solution environment at room temperature for 10,000 hours with the paint film intact. DETAILED DESCRIPTION
[0022] The polymer carboxylic acid and modified polysiloxane can both achieve the purpose of the present invention by using the existing technology. In the embodiment of the present invention, the model of the modified polysiloxane is Deqian 903, and the model of the polymer carboxylic acid is Deqian 904.
[0023] Example 1
[0024] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 50% of a paint component and 50% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0025] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0026] 30% of chloroether resin, 20% of xylene, 3% of a mixture of polymer carboxylic acid and modified polysiloxane, 1% of polyamide wax, 25% of pigment red iron oxide, 1% of T-12 organotin drier, and 20% of butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0027] The preparation method of the weather-resistant and alkali-resistant anticorrosive coating comprises the following steps:
[0028] (1) Adding chloroether resin, xylene, a mixture of high molecular weight carboxylic acid and modified polysiloxane, and polyamide wax while stirring at high speed, and stirring for 10 minutes after the mixing is completed, wherein the grinding is performed by using a horizontal sand mill to grind to a fineness of less than 30 nm, and then adding pigment, drying agent, and butyl acetate thereto, and stirring and mixing;
[0029] (2) Add the curing agent component to the product of step (1) and stir to mix.
[0030] Example 2
[0031] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 50% of a paint component and 50% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0032] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0033] 10% of chloroether resin, 40% of xylene, 0.2% of a mixture of polymer carboxylic acid and modified polysiloxane, 0.8% of polyamide wax, 40% of pigment red iron oxide, 1% of T-12 organotin drier, and 8% of butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0034] The preparation method of the weather-resistant and alkali-resistant anticorrosive coating comprises the following steps:
[0035] (1) Adding chloroether resin, xylene, a mixture of high molecular weight carboxylic acid and modified polysiloxane, and polyamide wax while stirring at high speed, and stirring for 30 minutes after the mixing is completed, wherein the grinding is performed by using a horizontal sand mill to grind the mixture to a fineness of less than 30 nm, and then adding pigment, drying agent, and butyl acetate, and stirring and mixing;
[0036] (2) Add the curing agent component to the product of step (1) and stir to mix.
[0037] Example 3
[0038] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 50% of a paint component and 50% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0039] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0040] 30% of chloroether resin, 34% of xylene, 0.2% of a mixture of polymer carboxylic acid and modified polysiloxane, 0.3% of polyamide wax, 15% of pigment red iron oxide, 0.5% of T-12 organotin drier, and 20% of butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0041] The preparation method is the same as Example 1.
[0042] Example 4
[0043] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 40% of a paint component and 60% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0044] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0045] 28% chloroether resin, 38% xylene, 0.2% mixture of polymer carboxylic acid and modified polysiloxane, 0.3% polyamide wax, 22% pigment red iron oxide, 0.5% T-12 organotin drier, 11% butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0046] The preparation method is the same as Example 1.
[0047] Example 5
[0048] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 40% of a paint component and 60% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0049] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0050] 16.7% of chloroether resin, 25% of xylene, 1.3% of a mixture of polymer carboxylic acid and modified polysiloxane, 1% of polyamide wax, 40% of pigment red iron oxide, 1% of T-12 organotin drier, and 15% of butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0051] The preparation method is the same as Example 1.
[0052] Example 6
[0053] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 40% of a paint component and 60% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0054] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0055] 13% chloroether resin, 30% xylene, 1.1% mixture of polymer carboxylic acid and modified polysiloxane, 0.3% polyamide wax, 40% pigment red iron oxide, 0.6% T-12 organotin drier, 15% butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0056] The preparation method is the same as Example 1.
[0057] Example 7
[0058] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 33% of a paint component and 67% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0059] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0060] 25% chloroether resin, 35% xylene, 0.5% mixture of polymer carboxylic acid and modified polysiloxane, 0.5% polyamide wax, 26.4% pigment red iron oxide, 0.6% T-12 organotin drier, 12% butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:1.
[0061] The preparation method is the same as Example 1.
[0062] Example 8
[0063] A weather-resistant and alkali-resistant anticorrosive coating, which, by weight percentage, consists of 33% of a paint component and 67% of a curing agent component; the curing agent component is hexamethylene diisocyanate;
[0064] Wherein, the paint component is composed of the following raw materials according to weight percentage:
[0065] 18% chloroether resin, 28% xylene, 0.6% mixture of polymer carboxylic acid and modified polysiloxane, 0.8% polyamide wax, 37% pigment red iron oxide, 0.6% T-12 organotin drier, 15% butyl acetate; wherein the weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:3.
[0066] The preparation method is the same as that of Example 1.
[0067] The properties of the coatings of Example 1, Example 4 and Example 7 were tested. The specific testing methods and results are shown in Table 1.
[0068] Table 1 Detection methods and results
[0069]
Claims
1. A weather-resistant and alkali-resistant anticorrosive coating, characterized in that: According to weight percentage, it is composed of 33-50% paint component and 50-67% curing agent component; Wherein, the paint component is composed of the following raw materials according to weight percentage: Chloroether resin 10-30%, xylene 20-40%, a mixture of high molecular weight carboxylic acid and modified polysiloxane 0.2-3%, polyamide wax 0.3-1%, pigment 15-40%, drier 0.1-1%, butyl acetate 8-20%; The curing agent component is hexamethylene diisocyanate; The weight ratio of the polymer carboxylic acid to the modified polysiloxane is 1:(1-3); The drier is T-12 organotin drier; The pigment is red iron oxide.
2. The weather-resistant and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The paint component is composed of the following raw materials in terms of weight percentage: 13-28% of chloroether resin, 25-38% of xylene, 0.2-1.3% of a mixture of polymer carboxylic acid and modified polysiloxane, 0.3-1% of polyamide wax, 22-40% of pigment, 0.5-1% of drying agent, and 11-15% of butyl acetate.
3. The weather-resistant and alkali-resistant anticorrosive coating according to claim 2, characterized in that: The paint component is composed of the following raw materials in terms of weight percentage: 18-25% of chloroether resin, 27-35% of xylene, 0.5-1.3% of a mixture of polymer carboxylic acid and modified polysiloxane, 0.3-0.8% of polyamide wax, 22-37% of pigment, 0.6-1% of drying agent, and 12-15% of butyl acetate.
4. The method for preparing the weather-resistant and alkali-resistant anticorrosive coating according to claim 1, characterized in that: The following steps are involved: (1) Add chloroether resin, xylene, a mixture of high molecular weight carboxylic acid and modified polysiloxane, and polyamide wax while stirring and mixing. After the mixing is completed, continue stirring for 10-30 minutes, grind, and then add pigment, drying agent, and butyl acetate, and stir and mix; (2) Add the curing agent component to the product of step (1) and stir to mix.
5. The method for preparing the weather-resistant and alkali-resistant anticorrosive coating according to claim 4, characterized in that: The grinding is performed by using a horizontal sand mill to grind the powder to a fineness of less than 30 nm.