A kind of white nano calcium carbonate and preparation method thereof

White nano calcium carbonate was produced by synchronous metathesis coating method of sterilization and coating CaCO3 crystal nuclei with humic acid in sterilization, solving the problems of energy waste, whiteness reduction and environmental pollution in nano calcium carbonate production, achieving high efficiency and environmental protection Preparation of white nano calcium carbonate.

CN116462218BActive Publication Date: 2024-11-08LINHAI BIOENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310239254.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-08
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

The existing nano calcium carbonate production methods have problems such as waste of energy, increased material consumption and reduced whiteness. The bleach is corrosive and costly, and the asynchronous coating process leads to environmental pollution.

Method used

Using sterilization liquid as raw material, white nano calcium carbonate is produced by synchronous metathesis coating method, and soluble humic acid in sterilization liquid is used to coat CaCO3 crystal nuclei to prevent agglomeration, and carbonize with high temperature through air or oxygen-enriched fluidization to achieve white nano calcium carbonate Preparation.

Benefits of technology

It realizes efficient preparation of white nano calcium carbonate, with narrow and uniform particle size distribution, easy separation and drying, and a whiteness of 90.4%, avoiding pollution and cost problems of bleaching method, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116462218B_ABST
    Figure CN116462218B_ABST
Patent Text Reader

Abstract

The invention provides a white nano calcium carbonate and a preparation method thereof. The preparation method comprises the following steps: S1, performing solid-liquid separation on biogas slurry water, and collecting separated liquid; S2, determining the alkalinity molar concentration of the biogas slurry water separated liquid in step S1, and determining the pH value of the separated liquid; S3, calculating the theoretical dosage of CaO according to the alkalinity molar concentration in the step; S4, adding CaO to the biogas slurry water separated liquid in step S1 according to the theoretical dosage of CaO, stirring until flocculent precipitation is generated, and preparing a humic acid-based nano calcium carbonate crude extract; S5, centrifuging the humic acid-based nano calcium carbonate crude extract, collecting the precipitate, drying, and carbonizing at 700-825° C. for 2-4 hours in air or oxygen-enriched fluidized state to obtain the white nano calcium carbonate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional material development, and in particular to white nano calcium carbonate and a preparation method thereof. Background Art

[0002] Nano calcium carbonate is a new type of ultrafine solid material, which is divided into calcite, aragonite, vaterite and amorphous crystal structures. Among them, calcite has the most stable thermodynamics, and amorphous is the most unstable. It appears relatively short-lived and becomes the seed for the growth of the other three crystal forms. Its particle size is between 10 and 100nm, and its specific surface area is between 18 and 90m2 / g. The particle size and specific surface area are approximately 1 / 10 and 8 times that of ordinary light calcium carbonate, showing small size effect, surface effect, macro quantum tunnel effect and quantum size effect. High porosity, high specific surface area, non-toxicity and biocompatibility make nano calcium carbonate have a wide range of industrial applications. Nano calcium carbonate is an excellent white reinforcing material in the rubber and plastic industries, which can make the product surface bright, with high tension resistance, bending resistance and good crack resistance. In the coatings and high-grade ink industries, it is used as a filler to reduce costs while improving product performance and playing a role in thickening and anti-settling. In the feed industry, it is used as a calcium supplement to increase the calcium content. In cosmetics, it can replace expensive titanium dioxide to meet the requirements of product purity, whiteness and fineness.

[0003] At present, the main method for preparing nano calcium carbonate is carbonization. The carbonization method relies on abundant mineral resources to calcine and generate CaO and CO2. CaO and H2O generate lime milk, and CO2 is introduced to carbonize it into CaCO3. The advantages of this method are: simple and easy to operate, environmentally friendly, and easy to produce on a large scale in industry. The disadvantages of the carbonization method are: the reaction process releases a lot of heat, and a condensing device needs to be added to maintain the reaction at room temperature, which increases production costs and wastes energy; and because low-concentration Ca(OH)2 participates in the reaction, material consumption increases and the production energy of the reaction equipment is weakened.

[0004] Nano calcium carbonate itself is white. The raw material limestone contains colored minerals such as iron, which reduces the whiteness of the light calcium. In the production process, colored substances such as organic matter and carbon particles are mixed in, which reduces the whiteness of the product. In order to improve the whiteness of nano calcium carbonate, a bleaching method is often used, that is, adding bleaching agents such as hydrogen peroxide (H2O2) and sodium hypochlorite (NaClO) to the digestion, carbonization or cooked slurry, adjusting the pH, and selecting appropriate temperature, concentration, and reaction time conditions to remove colored ions or substances in the raw material liquid. When H2O2 bleaching agent is selected, it can be converted into peroxy hydroxide ions (OOH - , HO2 - ), HO2 -Ions are active bleaching ions that can depolymerize lignin and produce carbonyl groups, and mainly react with conjugated carbonyl structures to destroy chromophores. The pH control range of H2O2 bleaching is 10.5-11.5, the temperature is between 65-80°C, and the bleaching time is inversely proportional to the consumption rate of H2O2. However, the bleaching method has the following disadvantages: the bleaching agent is corrosive, has high requirements for equipment, and the cost of the bleaching agent is high. The bleaching process is affected by pH, material slurry mass fraction, temperature, bleaching agent dosage, and bleaching time, and is prone to secondary wastewater problems. The one-step carbonization method in air or oxygen-enriched fluidized state to obtain white nano calcium carbonate can overcome the defects of the bleaching method for preparing white nano calcium carbonate, but this bleaching method has not been reported.

[0005] The existing simultaneous coating process for the production of nano calcium carbonate is to fill the polymer aggregates while the inorganic precursor chemically synthesizes the nano calcium carbonate particles in a mixed system of polymer coating and inorganic precursor solvent for synthesizing nano calcium carbonate. For example, polysaccharides and protein macromolecular polymers are used as heterogeneous substrates or adsorbed pre-nucleation clusters to regulate the nucleation of calcium carbonate. Humic acid is added to the system of preparing calcium carbonate by carbonization of Ca(OH)2 to regulate the microcrystalline morphology of calcium carbonate and successfully synthesize calcium carbonate with a high specific surface area. Nano calcium carbonate is prepared by double decomposition reaction of Na2CO3 and CaCl2 in a mixed aqueous solution of polyvinyl pyrrolidone (PVP) and sodium dodecylbenzene sulfonate (SDBS) to obtain spherical nano calcium carbonate with good dispersibility. The advantage of this technology is that the presence of the polymer can effectively inhibit the growth and agglomeration of inorganic nanoparticles, thereby solving the shortcomings of uneven dispersion and easy agglomeration of nano powders in organic / inorganic composite materials. However, the disadvantage of this technology is that the polymer coating added in the mixed solvent is not thorough, and the residue in the reaction solution is bound to lead to incomplete solution treatment, causing environmental pollution problems.

[0006] Anaerobic fermentation of biogas slurry is rich in alkalinity (HCO3 -), and soluble calcium salts form a specific system, undergo double decomposition reaction, and make nano calcium carbonate crystals nucleate and grow. The advantages of double decomposition reaction are: the crystal form, morphology, and particle size of CaCO3 are easy to control, the reaction kinetics are controllable, and the particle size distribution of the obtained product particles is narrow and uniform, and separation and drying are convenient. At the same time, the biogas slurry contains rich soluble humic acid organic matter. When the double decomposition reaction produces CaCO3 crystal nuclei, humic acid coats the CaCO3 crystal nuclei, inhibits the combination of CaCO3 crystal nuclei, and prevents the agglomeration of CaCO3 crystals. The advantages of this technology are: 1) it can realize the resource utilization of biogas slurry and turn waste into treasure; 2) the soluble humic acid in biogas slurry is used to coat instead of commercially available polymers (polysaccharides, proteins, PVP, SDBS) to achieve macroscopic preparation of nano calcium carbonate, without generating waste liquid, and can prevent biogas slurry pollution, which is more ecological and environmentally friendly; 3) the presence of soluble humic acid can prevent the agglomeration of nano calcium carbonate crystals. So far, there has been no report on a method for producing white nano-calcium carbonate with good dispersibility by subjecting biogas slurry to a synchronous double decomposition and coating reaction with a soluble calcium salt and removing calcium carbonate impurities by high-temperature carbonization in an air fluidized state. Summary of the invention

[0007] In view of this, the present invention provides a white nano-calcium carbonate and a preparation method thereof. The present invention uses biogas slurry produced in the production process of biogas industry as raw material, and carries out the biogas slurry synchronous double decomposition coating method to produce white nano-calcium carbonate. Biogas slurry is the product of anaerobic fermentation of organic waste. Because anaerobic fermentation realizes the hydrolysis and transformation of organic matter, the wastewater contains high concentrations of ammonia nitrogen, bicarbonate ions and soluble humic acid, etc., and calcium agent is added to react to obtain humic acid-based nano-calcium carbonate first, and further air or oxygen-enriched fluidization high-temperature carbonization can obtain white nano-calcium carbonate.

[0008] The white nano calcium carbonate prepared from biogas slurry has easy-to-regulate crystal form, morphology and particle size, and controllable reaction kinetics, so that the obtained product particles have narrow and uniform particle size distribution, and are easy to separate and dry. When the double decomposition reaction produces CaCO3 nuclei, humic acid coats the CaCO3 nuclei to inhibit the combination of CaCO3 nuclei and prevent the agglomeration of CaCO3 crystals. The prepared nano calcium carbonate is an excellent white reinforcing material in the rubber industry and plastics industry, which can make the surface of the products bright, with high tension resistance, bending resistance and good crack resistance. As a filler in the coating industry and high-grade ink industry, it can improve product performance and thicken and prevent sedimentation while reducing costs. In the feed industry, it is used as a calcium supplement to increase the calcium content. In cosmetics, it can replace high-priced titanium dioxide to meet the requirements of product purity, whiteness and fineness.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A method for preparing white nano calcium carbonate is provided, comprising the following steps:

[0011] S1, separating the biogas slurry into solid and liquid, and collecting the separated liquid;

[0012] S2, determining the alkalinity molar concentration of the biogas slurry water separation liquid in step S1, and determining the pH of the separation liquid;

[0013] S3, the theoretical dosage of CaO calculated according to the alkalinity molar concentration of the step;

[0014] S4, adding CaO according to the theoretical dosage of CaO to the biogas slurry water separation liquid in step S1, stirring until floccules are precipitated, and preparing a humic acid-based nano-calcium carbonate crude extract;

[0015] S5. Centrifuge the humic acid-based nano-calcium carbonate crude extract, collect the precipitate, dry it, and carbonize it at 700-825° C. for 2-4 hours in air or oxygen-enriched fluidized state to obtain the white nano-calcium carbonate.

[0016] Step S2 is specifically as follows:

[0017] Determine the alkalinity molar concentration of the biogas slurry water separation liquid in step S1 according to equations (1) and (2);

[0018]

[0019]

[0020] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.

[0021] Step S3 is specifically as follows:

[0022] According to the molar concentration of alkalinity of the biogas slurry in step S2, the theoretical dosage of CaO is calculated according to the double decomposition reaction formula (3), (4) and formula (5); wherein the dosage of CaO is such that the pH of the biogas slurry reaction is maintained in the range of 8.70 to 8.99;

[0023] When Ca(OH)2 is insufficient: Ca()2+2NH4HCO3→CaCO3↓+(4)2CO3+2H2O(3)

[0024] When Ca(OH)2 is sufficient: Ca()2+H4HCO3→CaCO3↓+NH3↑+2H2O(4)

[0025]

[0026] m CaO = CaO ×CCaO ×V 沼液反应体积 (6)

[0027] Among them, C CaO Indicates the molar concentration of CaO added, mol / L; M CaO represents the molar mass concentration of CaO, 56 g / mol; V 沼液反应体积 Indicates the total volume of the biogas slurry reaction, L; m CaO Indicates the theoretical added mass of CaO, g.

[0028] In step S3, according to the molar concentration of alkalinity of the biogas slurry in step S2, the molar ratio of Ca(OH)2 / NH4HCO3 is 1:2 according to the double decomposition reaction formula (3), and the theoretical dosage of CaO is calculated according to formula (5). The amount of Ca(OH)2 cannot be excessive, see reaction (4), that is, the amount of CaO added to the biogas slurry is required to maintain the pH in the range of 8.70 to 8.99, because the excess Ca(OH)2 makes the pH reach 9 to 14, causing the ammonium ions (NH4 + ) and hydroxide (OH - ) reacts to generate ammonia water (NH3·H2O), which volatilizes in the form of ammonia gas (NH3), resulting in the loss of nitrogen in the biogas slurry and affecting the recovery of nitrogen resources in the biogas slurry. Therefore, the molar ratio of Ca(OH)2 / NH4HCO3 is controlled at ≤1, and the optimal molar ratio is 0.5.

[0029] The method for preparing white nano calcium carbonate by the biogas slurry synchronous double decomposition coating method further comprises step S6, wherein step S6 comprises the following steps:

[0030] S61, centrifuging the humic acid-based nano-calcium carbonate crude extract of step S4, collecting the supernatant into a dry container, measuring the pH of the supernatant, and titrating the alkalinity of the biogas slurry with an acid solution according to formula (8) and formula (9). When the methyl orange indicator changes from orange to orange, the titration is stopped and the titrated acid (H + ) volume △V, and the carbonate (CO3 2- ) molar concentration;

[0031] S62, according to reaction formula (10) and reaction formula (11), calculate the theoretical molar concentration value of CaCl2 to be added;

[0032] S63. Calculate the theoretical dosage of CaCl₂ according to Reaction Formula (12); add CaCl₂ to the supernatant, and control the pH at 7.0 - 7.5 at the end of the reaction; according to Reaction Formula (13), continue to adjust with NaOH solution until the pH rises to about 8.3 - 8.5, stop adding NaOH solution, stir for 10 - 20 min, let stand for 10 - 20 min, flocculent precipitate appears, collect the precipitate, dry it, and carbonize it at 700 - 825 °C for 2 - 4 h in air or oxygen-rich fluidized state to obtain the white nano calcium carbonate;

[0033]

[0034]

[0035] CaCl₂ + (NH₄)₂CO₃ → CaCO₃↓ + 2NH₄Cl (10)

[0036]

[0037]

[0038] 2NaOH + Ca(HCO₃)₂ → CaCO₃↓ + Na₂CO₃ + 2H₂O (13)

[0039] Among them, represents the molar concentration of carbonate, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the centrifuged collected liquid, L; represents the molar concentration of calcium chloride, mol / L; represents the molar mass concentration of calcium chloride (111 g / mol), g / mol; V 分离上清液 represents the total volume of the centrifuged supernatant, L; represents the theoretical k = 1 dosage mass of calcium chloride or the actual dosage mass with 0.5 < k < 1, g.

[0040] In Reaction Formulas (3) and (4), the molar ratio of Ca(OH)₂ / NH₄HCO₃ is controlled at 0.5 - 1.

[0041] In step S5, the drying conditions are: drying in an oven at 100 - 140 °C for 8 - 12 h.

[0042] The biogas slurry water is the biogas slurry water from the anaerobic fermentation tank of the Miaoji Biogas Station in Funan County, Anhui Province

[0043] In step S1, the solid-liquid separation of the biogas slurry water is carried out by a spiral press filter.

[0044] As an embodiment of the present invention, step S6 is specifically as follows:

[0045] Centrifuge the crude extract of humic acid-based nano-calcium carbonate in step S4, collect the supernatant into a dry beaker, measure the pH of the collected liquid to be pH = 8.799, and continue to stir on a magnetic stirrer at a rotation speed of 500 r / min; according to the product (NH4)2CO3 in reaction formula (3), take 1 mL of the supernatant, and according to formulas (8) and (9), titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl. When the methyl orange indicator changes from orange-yellow to orange-red, stop the titration and record the volume of the titrant acid (H + ) △V, and calculate the molar concentration of carbonate (CO3 2- ); according to reaction formula (10), the molar ratio of CaCl2 / CO3 2- is 1:1, and according to reaction formula (11), calculate the theoretical molar concentration value of the CaCl2 to be added; according to reaction formula (12), when the dosing coefficient k = 1, calculate the theoretical dosing amount of CaCl2; because CaCl2 belongs to a strong acid and weak base salt, the free Ca 2+ combines with HCO3 - to cause the hardness of the collected liquid to be too high; to reduce the hardness in the collected liquid, according to reaction formula (12), with the dosing coefficient 0.5 < k < 1, calculate the actual dosing amount of CaCl2; add the actual dosing amount of CaCl2 to the supernatant, and control the pH at the end of the reaction in the range of 7.0 - 7.5; according to reaction formula (13), continue to use 2 mol / L NaOH (AR) solution for callback. Insert the pH meter electrode into the reaction beaker to monitor the pH value in real time. When the pH rises to about 8.3, stop adding the NaOH solution, start recording the magnetic stirring time for 10 min, keep the pH stable, and let it stand for 20 min. As a result, the pH reaches 8.357 and the hardness reduction rate reaches 90.47%. That is, the NaOH is callback to control the final pH of the reaction solution in the range of 8.3 - 8.5, and a flocculent precipitation phenomenon appears. Collect the precipitate, dry it, and under air or oxygen-rich fluidized state, carbonize it at 700 - 825 °C for 2 - 4 h to obtain the white nano-calcium carbonate;

[0046]

[0047]

[0048] CaCl2 + (NH4)2CO3 → CaCO3↓ + 2NH4Cl (10)

[0049]

[0050]

[0051] 2NaOH + Ca(HCO3)2 → CaCO3↓ + Na2CO3 + 2H2O (13)

[0052] Among them, represents the molar concentration of carbonate, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the centrifuged collected liquid, L; represents the molar concentration of calcium chloride, mol / L; represents the molar mass concentration of calcium chloride (111 g / mol), g / mol; V 分离上清液 is the total volume of the separated supernatant, L; represents the theoretical k = 1 dosing mass of calcium chloride or the actual dosing mass when 0.5 < k < 1, g.

[0053] The white nanometer calcium carbonate obtained by the preparation method of the white nanometer calcium carbonate also belongs to the protection scope of the present invention.

[0054] The present invention also claims to protect an application of the said white nanometer calcium carbonate in rubber, plastic, coating, ink, feed, and cosmetics.

[0055] Compared with the prior art, the advantages of the present invention are as follows:

[0056] 1) Design the OH formed by the CaO emulsion - The strong electrolyte reacts with the weak electrolyte HCO3- in biogas slurry to generate CO3 2- , and further reacts with Ca 2+ ions to generate CaCO3 precipitate, solving the problems of low conductivity and high energy consumption caused by the influence of the weak electrolyte HCO3 - in biogas slurry on the process of recovering nitrogen and potassium resources from biogas slurry by electrodialysis.

[0057] 2) The biogas slurry reacts with CaO to produce flocculent precipitates, and the solid-liquid separation supernatant further reacts with CaCl2. The flocculent precipitate of the reaction is adjusted back with NaOH to obtain humic acid-based nanometer calcium carbonate. The precipitate is dried, fluidized by air or oxygen-enriched air, and carbonized at 700 °C for 2 h to obtain white nanometer calcium carbonate. The first-step white burning method overcomes the disadvantages of the bleaching method: that is, the bleaching agent is corrosive, has high requirements for equipment, and the cost of the bleaching agent is high. The bleaching process is affected by pH, the mass fraction of the material slurry, temperature, the dosage of the bleaching agent, and bleaching time, and it is easy to produce the problem of secondary wastewater.

[0058] 3) The theory and method of synchronous double decomposition coating were proposed to prepare nano calcium carbonate in biogas slurry. Because the double decomposition method is a liquid-liquid reaction between a soluble calcium agent and soluble carbonates and bicarbonates to produce calcium carbonate. Compared with the carbonization method, the advantages of this method are fast reaction rate, high efficiency, controllable reaction conditions, and easy to study the laws of reaction kinetics; at the same time, the soluble humic acid in the biogas slurry contains carboxyl, hydroxyl and other groups; according to the double layer theory, the double layer of soluble humic acid organic matter still maintains electrical neutrality, but the number of positive ions decreases, that is, the thickness of the double layer becomes thinner, and the ξ potential on the sliding surface of the soluble humic acid organic matter is reduced to the critical potential ξ K , repulsive barrier E max The humic acid is reduced to zero, and the humic acid is destabilized and condensed. A large number of calcium carbonate microcrystals appear in the double decomposition reaction, and the Ca atoms in the surface molecules can easily chelate with the O atoms in the -OH and -COOH on the humic acid chain. The soluble humic acid in the biogas slurry is used to coat the calcium carbonate microcrystals, which has a strong molecular binding ability. The humic acid coating also prevents the agglomeration of the calcium carbonate crystals, thus overcoming the defects of the asynchronous coating method.

[0059] 4) This study reports for the first time the use of soluble humic acid organic matter in biogas slurry to coat nano calcium carbonate generated by double decomposition. Through a one-step calcination method, the whiteness value of nano calcium carbonate reaches 90.4; and the soluble humic acid coating prevents the nano calcium carbonate from agglomerating. Under high temperature of 700℃~825℃ in air or oxygen-enriched fluidization for 2~4h, the soluble humic acid organic matter is released in the form of gas, which is beneficial to the dispersion of calcium carbonate. The nano calcium carbonate is spindle-shaped, needle-shaped, and rod-shaped.

[0060] 5) The biogas slurry is used to prepare white nano-calcium carbonate through a synchronous double decomposition coating method, thus realizing the resource utilization of the biogas slurry and turning waste into treasure.

[0061] 6) Soluble humic acid in biogas slurry is used to coat and replace commercially available polymers (polysaccharides, proteins, PVP, SDBS) to achieve macroscopic preparation of nano calcium carbonate, which does not produce waste liquid, can prevent biogas slurry pollution, and is more ecological and environmentally friendly.

[0062] 7) A one-step bleaching method, i.e., 700°C high temperature conditions, was used to obtain white nano calcium carbonate, the whiteness of which was 15.5% higher than that of the sample obtained by the bleaching method, and reached 90.4% of the reference value of "Nano Calcium Carbonate" (GB / T 19590-2011). The SEM analysis results showed that the bleached nano calcium carbonate was needle-shaped, rod-shaped, and spindle-shaped, with a certain degree of dispersion, and the particle size was between the nanometer and micrometer scales. The particle size distribution results showed that compared with the commercially available nano calcium carbonate, the bleached white nano calcium carbonate accounted for more than 50% of the particle distribution with a smaller particle size. The XRD analysis results showed that the bleached white nano calcium carbonate was in the calcite crystal form, and XRF further proved that it was calcium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0064] Figure 1 The diagram is a mechanism diagram of preparing white nano calcium carbonate by synchronous double decomposition coating principle and method of biogas slurry and calcium agent (CaO, CaCl2) of the present invention;

[0065] Figure 2 This is the reaction process and product result diagram of the experiment of preparing white nano calcium carbonate from biogas slurry;

[0066] Figure 3 As: the morphology result of white nano calcium carbonate;

[0067] Figure 4 The figure is: the particle size distribution result of white nano calcium carbonate;

[0068] Figure 5 : XRD crystal phase analysis results of white nano calcium carbonate. DETAILED DESCRIPTION

[0069] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0070] The biogas slurry treated in the experimental process comes from the anaerobic fermentation tank effluent of Miaoji Biogas Station (32°38′7.68″N, 115°43′3.24″E) in Funan County, Fuyang City, Anhui Province, and the liquid separated by solid-liquid separation by the snail stacker. During the test period (April 1, 2022 to October 14, 2022), the COD of the biogas slurry was 4063-5207 mg / L, and the NH4 + -N is 2424~3024mg / L, containing HCO3 - The total alkalinity of ions (calculated as CaCO3) is 8759~14264 mg / L, the hardness (calculated as CaCO3) is 70~220 mg / L, the pH is 8.113~8.327, and the water temperature is 14.1~29.4℃.

[0071] The reagents required for the test process: calcium chloride, calcium oxide, sodium hydroxide, pure sodium carbonate, hydrogen peroxide, anhydrous ethanol, and hydrochloric acid, all of which are AR grade.

[0072] Synchronous metathesis coating theory, mixing organic polymers with inorganic precursors in a solvent, so that the inorganic precursors chemically synthesize nanoparticles and fill them into polymer aggregates at the same time. The presence of polymers can effectively control the particle size growth of inorganic nanoparticles and prevent the agglomeration of nanoparticles; the mechanism of preparing white nano calcium carbonate from biogas slurry, see Figure 1 .

[0073] Example 1 Preparation of white nano calcium carbonate

[0074] This embodiment provides a method for preparing white nano calcium carbonate, comprising the following steps:

[0075] Step 1, specifically taking the biogas slurry water from the anaerobic fermentation tank of Miaoji Biogas Station in Funan County, Anhui Province as an example, the biogas slurry water from the anaerobic fermentation tank first passed through a screw stacker for solid-liquid separation, and the pH of the separated liquid was measured to be 8.223.

[0076] Step 2: Take the separated liquid biogas slurry V = 1 mL from step 1 above and put it into a 250 mL clean conical flask, dilute it 50 times with distilled water, add 4 drops of methyl orange indicator, and according to the reaction principle, see formula (1), titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl. When the methyl orange indicator changes from orange to orange, stop the titration and record the titrated acid (H + ) volume △V = 3.75mL; According to equation (2), the alkalinity of the biogas slurry is calculated to be 0.1875mol / L;

[0077]

[0078]

[0079] in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; It represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the biogas slurry sample, L.

[0080] Step 3, according to the biogas slurry after solid-liquid separation in the above step 1, take 1 mL of the biogas slurry into a colorimetric tube, dilute it to 10 mL with distilled water, and use the "Technical Requirements and Detection Methods for COD Photometric Rapid Determination Instrument" (HJ 924-2017) and a multi-parameter water quality analyzer (5B-3B (V8), Lianhua Technology Co., Ltd.) to perform spectrophotometric determination of the soluble humic acid organic matter in the biogas slurry, which is 2678 mg / L (in terms of chemical oxygen demand (COD)).

[0081] Step 4, according to the molar concentration of alkalinity of the biogas slurry in step 2, according to the double decomposition reaction formula (3), the molar ratio of Ca(OH)2 / NH4HCO3 is 1:2, and the theoretical dosage of CaO calculated according to formula (5) is 0.09375mol / L. The amount of Ca(OH)2 cannot be excessive. The pH of the solution after the reaction with Ca(OH)2 should be controlled in the range of 8.7 to 8.99, see reaction (4), because the excess Ca(OH)2 makes the pH of the reaction solution in the range of 9 to 14. Under strong alkaline conditions, the free ammonium ions (NH4 + ) and hydroxide ions (OH - ) ion reaction produces ammonia water (NH3·H2O), which is easily volatilized into ammonia gas (NH3), resulting in the loss of biogas liquid nitrogen resource recovery. Therefore, the molar ratio of Ca(OH)2 / NH4HCO3 is controlled in the range of 0.5-1, and the optimal molar ratio is 0.5;

[0082] Ca(OH)2+2NH4HCO3→CaCO3↓+(NH4)2CO3+2H2O(when Ca(OH)2 is insufficient) (3)

[0083] Ca(OH)2+NH4HCO3→CaCO3↓+NH3↑+2H2O (when Ca(OH)2 is sufficient) (4)

[0084]

[0085] m CaO =M Cao ×C cao ×V 沼液反应体积 (6)

[0086] Among them, C CaO Indicates the molar concentration of CaO added, mol / L; M CaO represents the molar mass concentration of CaO, 56 g / mol; V 沼液反应体积 is the total volume of biogas slurry reaction, L; m Cao Indicates the theoretical added mass of CaO, g.

[0087] Step 5. According to steps 3 and 4, pour 1L of the biogas slurry from step 1 into a clean beaker and place it on a magnetic stirrer with stirring at a speed of 500r / min. According to the theoretical CaO molar dosage of 0.09375mol / L, the added mass of CaO(AR) is calculated to be 5.25g according to formula (6). According to reaction formula (7), prepare a 10% Ca(OH)2 emulsion with distilled water. Use a glass rod to drain the Ca(OH)2 emulsion and slowly add it to the beaker. Start timing when the emulsion is added. Stir magnetically for 10 minutes and let it stand for 20 minutes. After reacting with the Ca(OH)2 emulsion, the pH of the reaction liquid is controlled in the range of 8.7 to 8.99. During the stirring process, a flocculent substance precipitates. According to the double decomposition reaction formula (3) and the synchronous double decomposition coating theory, while the CaCO3 precipitate is produced, the biogas soluble humic acid coats the CaCO3 crystal nucleus to form humic acid-based nano-calcium carbonate. Record sample 1. Figure 2 ;

[0088] CaO+H2O→Ca(OH)2 (7).

[0089] Step 6, centrifuging the humic acid-based nano-calcium carbonate sample 1 of step 5 to separate the solid from the liquid, placing the solid after the solid-liquid separation in an oven at 105° C. and drying for 10 hours, and cooling.

[0090] Step 7, pour the humic acid-based nano-calcium carbonate dried sample of step 6 into a semicircular crucible, put it into a muffle furnace or a converter, introduce air or oxygen-enriched fluidized state, carbonize at 700°C for 2h, cool, and obtain white nano-calcium carbonate (sample 1 final product), see Figure 2 .

[0091] Step 8, according to step 6, collect the centrifuged liquid of sample 1 into a dry beaker, measure the pH value of the collected liquid to be 8.799, continue to stir on a magnetic stirrer, and rotate at a speed of 500 r / min; according to the product (NH4)2CO3 of reaction formula (3), take 1 mL of the collected liquid, and titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl according to formula (8) and formula (9). When the methyl orange indicator changes from orange to orange, stop the titration and record the titrated acid (H + ) volume △V = 3.6mL, and the carbonate (CO3 2- ) has a molar concentration of 0.09 mol / L; According to reaction formula (10), CaCl2 / CO3 2- The molar ratio is 1:1. According to reaction formula (11), the theoretical molar concentration of CaCl2 to be added is 0.09 mol / L. According to reaction formula (12), when the addition coefficient k = 1, the theoretical addition amount of CaCl2 is 9.99 g. Because CaCl2 is a strong acid and weak base salt, the free Ca 2+ With HCO3 -Combination leads to too high hardness of the collected liquid. To reduce the hardness in the collected liquid, according to Reaction Formula (12), the addition coefficient is 0.5 < k < 1. The optimal value of the addition coefficient in this embodiment is k = 0.9375. The actual addition value of CaCl2 is 9.3656 g, which is prepared into a 35% CaCl2 solution with distilled water and slowly added to the beaker through a glass rod. After adding, start recording the magnetic stirring time for 10 min, let it stand for 20 min, and measure the pH = 7.233. When the reaction with CaCl2 ends, it is within the control range of pH 7.0 - 7.5. According to Reaction Formula (13), continue to use 2 mol / L NaOH (AR) solution for callback. The pH meter electrode is inserted into the reaction beaker to monitor the pH value in real-time. When the pH rises to about 8.3, stop adding the NaOH solution, start recording the magnetic stirring time for 10 min, keep the pH stable, let it stand for 20 min, and the result shows that the pH reaches 8.357. After using NaOH to callback the reaction solution, the pH of the solution should be controlled within the range of 8.3 - 8.5. The hardness is reduced from 1313.18 mg / L to 125.11 mg / L, and the hardness reduction rate reaches 90.47%. Similar to the result of Step 5, there is a phenomenon of flocculent precipitation. According to Reaction Formulas (10) and (13) and the synchronous metathesis coating theory and method, it is humic acid-based nano calcium carbonate. Record Sample 2, see Figure 2 。

[0092]

[0093]

[0094] CaCl2+(NH4)2CO3→CaCO3↓+2NH4Cl (10)

[0095]

[0096]

[0097] 2NaOH+Ca(HCO3)2→CaCO3↓+Na2CO3+2H2O (13)

[0098] Among them, represents the molar concentration of carbonate, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the centrifuged collected liquid taken, L; represents the molar concentration of calcium chloride, mol / L; V 分离上清液 represents the volume of the separated supernatant, L; represents the molar mass concentration of calcium chloride (111 g / mol), g / mol; Indicates the theoretical k = 1 dosing mass of calcium chloride or the actual dosing mass with 0.5 < k < 1, g.

[0099] Step 9: Centrifuge the humic acid-based nano calcium carbonate sample 2 from Step 8 for solid-liquid separation. Place the separated solid in an oven and dry it at 105 °C for 10 h, then cool it.

[0100] Step 10: Pour the dried humic acid-based nano calcium carbonate sample from Step 9 into a semi-circular crucible, place it in a muffle furnace or rotary furnace, introduce air or in an oxygen-enriched fluidized state, carbonize it at 700 °C for 2 h, then cool it to obtain white nano calcium carbonate (the final product of sample 2), see Figure 2 .

[0101] Step 11: The whiteness of the final products of sample 1 and sample 2 from Step 7 and Step 10 both reach 90.4, with good dispersibility. The nano calcium carbonate is in the shape of needles, rods, and spindles.

[0102] Preparation of white nano calcium carbonate in Example 2

[0103] This example provides a method for preparing white nano calcium carbonate, which includes the following steps:

[0104] Step 1: Specifically, taking the biogas slurry water from the anaerobic fermentation tank of the Miaoji Biogas Station in Funan County, Anhui Province as an example, the biogas slurry water from the anaerobic fermentation tank first undergoes solid-liquid separation through a screw press, and the pH of the separated liquid is measured to be 8.304.

[0105] Step 2: Take 1 mL of the separated biogas slurry (V) from Step 1 and put it into a clean 250 mL conical flask, dilute it 50 times with distilled water, add 4 drops of methyl orange indicator. According to the reaction principle, see Equation (1), titrate the alkalinity of the biogas slurry with 0.05 mol / L HCl. When the methyl orange indicator changes from orange-yellow to orange-red, stop titration and record the titrated acid (H + ) volume ΔV = 3.5 mL; According to Equation (2), calculate the alkalinity of the biogas slurry to be 0.175 mol / L.

[0106]

[0107]

[0108] Among them, represents the molar concentration of the alkalinity of the biogas slurry, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titrated volume of the acid, L; V represents the volume of the biogas slurry sample taken, L.

[0109] Step 3, according to the biogas slurry after solid-liquid separation in the above step 1, take 1 mL of the biogas slurry into a colorimetric tube, dilute it to 10 mL with distilled water, and use the "Technical Requirements and Detection Methods for COD Photometric Rapid Determination Instrument" (HJ 924-2017) and a multi-parameter water quality analyzer (5B-3B (V8), Lianhua Technology Co., Ltd.) to perform spectrophotometric determination of the soluble humic acid organic matter in the biogas slurry, which is 2532 mg / L (in terms of chemical oxygen demand (COD)).

[0110] Step 4, according to the molar concentration of alkalinity of the biogas slurry in step 2, according to the double decomposition reaction formula (3), the molar ratio of Ca(OH)2 / NH4HCO3 is 1:2, and the theoretical dosage of CaO calculated according to formula (5) is 0.0875 mol / L. The amount of Ca(OH)2 cannot be excessive, see reaction (4), that is, the final pH of the reaction with the Ca(OH)2 emulsion is controlled in the range of 8.7 to 8.99, because excessive Ca(OH)2 makes the pH range of 9 to 14, which is a strong alkaline environment, which will cause the free ammonium ions (NH4 + ) and hydroxide ions (OH - ) reacts to produce ammonia water (NH3·H2O), which is easily volatilized and eventually leads to the loss of nitrogen resource recovery in the biogas slurry. Therefore, the molar ratio of Ca(OH)2 / NH4HCO3 is controlled in the range of 0.5 to 1, and the optimal molar ratio is 0.5.

[0111] Ca(OH)2+2NH4HCI3→CaCO3↓+(NH4)2CO3+2H2O(when Ca(OH)2 is insufficient)(3)

[0112] Ca(OH)2+NH4HCO3→CaCO3↓+NH3↑+2H2O (when Ca(OH)2 is sufficient) (4)

[0113]

[0114] m Cao =M CaO ×C Cao ×V 沼液反应体积 (6)

[0115] Among them, C CaO Indicates the molar concentration of CaO added, mol / L; M CaO represents the molar mass concentration of CaO, 56 g / mol; V 沼液反应体积 is the total volume of biogas slurry reaction, L; m CaO Indicates the theoretical added mass of CaO, g.

[0116] Step 5, according to steps 3 and 4, take 1L of the biogas slurry from step 1 and pour it into a clean beaker, and place it on a magnetic stirrer and stir it at a speed of 500r / min; according to the theoretical CaO molar dosage of 0.0875mol / L, the added mass of CaO(AR) is calculated to be 4.9g according to formula (6); according to reaction formula (7), use distilled water to prepare a 10% Ca(OH)2 emulsion; use a glass rod to drain the Ca(OH)2 emulsion and slowly add it to the beaker, start timing when the emulsion is added, stir magnetically for 10min, and let it stand for 20min. During the stirring process, a flocculent substance precipitates. According to the double decomposition reaction formula (3) and the synchronous double decomposition coating theory, when CaCO3 precipitation is generated, the biogas slurry soluble humic acid coats the CaCO3 crystal nucleus to form humic acid-based nano calcium carbonate, and record sample 1.

[0117] CaO+H2O→Ca(OH)2 (7)

[0118] Step 6, centrifuging the humic acid-based nano-calcium carbonate sample 1 of step 5 to separate the solid from the liquid, placing the solid after the solid-liquid separation in an oven at 105° C. and drying for 10 hours, and cooling.

[0119] Step 7, pour the humic acid-based nano-calcium carbonate dried sample of step 6 into a semicircular crucible, put it into a muffle furnace or a converter, introduce air or oxygen-enriched fluidized state, carbonize at 700°C for 2h, cool, and obtain white nano-calcium carbonate (sample 1 final product).

[0120] Step 8, according to step 6, collect the centrifuge of sample 1 into a dry beaker, measure the pH of the collected liquid to be 8.766, continue to stir on a magnetic stirrer, and rotate at 500r / min; according to the product (NH4)2CO3 of reaction formula (3), take 1mL of the collected liquid, and titrate the alkalinity of the biogas slurry with 0.05mol / L HCl according to formula (8) and formula (9). When the methyl orange indicator changes from orange to orange, stop the titration and record the titrated acid (H + ) volume △V = 3.6mL, calculate the bicarbonate (CO3 2- ) has a molar concentration of 0.09 mol / L; According to reaction formula (10), CaCl2 / CO3 2- The molar ratio is 1:1. According to reaction formula (11), the theoretical molar concentration of CaCl2 to be added is 0.09 mol / L. According to reaction formula (12), when the addition coefficient k = 1, the theoretical addition amount of CaCl2 is 9.99 g. Because CaCl2 is a strong acid and weak base salt, the free Ca 2+ With HCO3 -Combination leads to too high hardness of the collected liquid. To reduce the hardness in the collected liquid, according to reaction formula (12), the addition coefficient is 0.5 < k < 1. The optimal value of the addition coefficient in this embodiment is k = 0.765. The actual addition value of CaCl2 is 7.64 g, which is prepared into a 35% CaCl2 solution with distilled water and slowly added to the beaker through a glass rod. After adding, start recording the magnetic stirring time for 10 min, let it stand for 20 min, and measure the pH = 7.177, within the control range of 7.0 - 7.5 for the reaction solution pH after reacting with CaCl2. According to reaction formula (13), continue to use 2 mol / L NaOH (AR) solution for callback. Insert the pH meter electrode into the reaction beaker to monitor the pH value in real time. When the pH rises to about 8.3, stop adding the NaOH solution, start recording the magnetic stirring time for 10 min, keep the pH stable, let it stand for 20 min, and the result shows that the pH reaches 8.391, within the control range of 8.3 - 8.5 for the reaction solution pH after callback with NaOH. The hardness decreases from 1146.03 mg / L to 275.25 mg / L, and the hardness reduction rate reaches 75.98%. Similar to the result of step 5, a flocculent precipitation phenomenon appears. According to reaction formulas (10) and (13) and the synchronous double decomposition coating theory and method, it is humic acid-based nano calcium carbonate, and sample 2 is recorded.

[0121]

[0122]

[0123] CaCl2+(NH4)2CO3→CaCO3↓+2NH4Cl (10)

[0124]

[0125]

[0126] 2NaOH+Ca(HCO3)2→CaCO3↓+Na2CO3+2H2O (13)

[0127] Among them, represents the molar concentration of carbonate, mol / L; represents the molar concentration of the known acid, mol / L; ΔV represents the titration volume of the acid, L; V represents the volume of the centrifuged collected liquid taken, L; represents the molar concentration of calcium chloride, mol / L; represents the molar mass concentration of calcium chloride (111 g / mol), g / mol; V 分离上清液 represents the total volume of the separated supernatant, L; represents the theoretical k = 1 addition mass of calcium chloride or the actual addition mass of 0.5 < k < 1, g.

[0128] Step 9, centrifuging the humic acid-based nano-calcium carbonate sample 2 of step 8 to separate the solid from the liquid, placing the solid after the solid-liquid separation in an oven at 105° C. and drying for 10 hours, and cooling.

[0129] Step 10, pour the humic acid-based nano-calcium carbonate dried sample of step 9 into a semicircular crucible, put it into a muffle furnace or a converter, introduce air or oxygen-enriched fluidized state, carbonize at 700°C for 2h, cool, and obtain white nano-calcium carbonate (sample 2 final product).

[0130] Step 11, the final products of sample 1 and sample 2 in step 7 and step 10 have a whiteness of 90.4, good dispersibility, and the nano calcium carbonate is in the shape of needles, rods and spindles.

[0131] Comparative Example 1

[0132] The difference between this comparative example and Example 1 is that in step 7, carbonization is carried out under anaerobic conditions, specifically:

[0133] Step 7: Replace with humic acid-based nano-calcium carbonate. Pour the dried sample into a semicircular crucible, put it into a muffle furnace or a converter, and carbonize it at 700°C for 2 hours without oxygen to obtain black conductive nano-calcium carbonate, not white nano-calcium carbonate.

[0134] Comparative Example 2

[0135] The difference between this comparative example and Example 1 is that step 7 is specifically as follows:

[0136] The humic acid-based nano-calcium carbonate dry sample is poured into a semicircular crucible, placed in a muffle furnace or a converter, and fluidized with nitrogen (N2), and carbonized at 700°C for 2h to obtain black conductive nano-calcium carbonate, non-white nano-calcium carbonate.

[0137] Comparative Example 3

[0138] The difference between this comparative example and Example 1 is that step 7 is specifically as follows: the humic acid-based nano-calcium carbonate dry sample is poured into a semicircular crucible, placed in a muffle furnace or a converter, and carbon dioxide (CO2) is introduced for fluidization, and carbonized at 700°C for 2h to obtain black conductive nano-calcium carbonate, non-white nano-calcium carbonate.

[0139] Comparative Example 4

[0140] The difference between this comparative example and Example 1 is that step 7 is specifically as follows:

[0141] The humic acid-based nano-calcium carbonate dry sample is poured into a semicircular crucible, placed in a muffle furnace or a converter, introduced with air for fluidization, and carbonized at 550° C. for 4 hours to obtain black conductive nano-calcium carbonate, non-white nano-calcium carbonate.

[0142] Comparative Example 5

[0143] The difference between this comparative example and Example 1 is that the one-step 700°C high temperature carbonization bleaching method is replaced by a bleaching method, that is, the precipitate sample of the reaction of biogas slurry and CaCl2, and the precipitate sample of the reaction of the separation liquid of the former reaction with CaO and NaOH, the two are mixed with about 50mL, first soaked with 15% Na2CO3 solution 100mL, the solution changes from light yellow to tea red, and the solution is removed. Then, the solid is washed with pure water, each time with 100mL of pure water, and the cleaning liquid stops from brown to colorless, and a total of 7 washings. After washing, the remaining solid 40mL is repeatedly soaked with anhydrous ethanol, the first ethanol consumption is 200mL, the soaking time is 20min, the second consumption is 160mL, the soaking time is 11min, the third and fourth consumptions are 80mL, the soaking time is 11min, and the soaking liquid changes from yellow to clear and transparent. The solid is filtered, placed in a 105°C oven and dried for 66min, and cooled. Then 30 mL of the dried sample was bleached with 200 mL of 30% H2O2 for 4 h. Washed with pure water and filtered twice, washed with anhydrous ethanol twice, filtered, put into an oven at 105°C for 2 h, cooled, and obtained white nano calcium carbonate. The whiteness of the final sample was 68.2 as measured by a whiteness meter (model WSB-1, Hangzhou Caipu Technology Co., Ltd.), which is 78.2% of the standard whiteness, 12.2% lower than the whiteness of the one-step bleaching method. In addition, the bleaching agent is corrosive, has high requirements for equipment, and has high bleaching agent costs. The bleaching process is affected by pH, material slurry mass fraction, temperature, bleaching agent dosage, and bleaching time, and is prone to secondary wastewater problems.

[0144] Comparative Example 6

[0145] The difference between this comparative example and Example 1 is that the one-step 700°C high temperature carbonization bleaching method is replaced by a bleaching method, that is, 50mL of the precipitate sample of the reaction of biogas slurry with CaCl2 and 45mL of the precipitate sample of the reaction of the separated liquid of the former reaction with CaO and NaOH, the former is impregnated twice with 10% NaOH solution at a volume ratio of 1:1, the impregnation time is 70min and 30min respectively, and the impregnation liquid is yellow; the latter is impregnated twice with 15% Na2CO3 solution at a volume ratio of 1:2, the impregnation time is 70min and 30min respectively, and the impregnation liquid changes from brown to milky yellow. The precipitate sample is retained, and the former and the latter are bleached with 15% H2O2 at a volume ratio of 1:2 respectively, put into a water bath (model HH-420, Shanghai Lichen Bangxi Instrument Technology Co., Ltd.) at a constant temperature of 65°C for 2h, and stand for 4h. The bleaching liquid is yellow and light yellow respectively, and the solid-liquid separation is achieved. Take 10mL of the former precipitate sample and 15mL of the latter precipitate sample, wash them twice with pure water at a volume ratio of 1:5 and 1:3 respectively, each washing time is 30min, and the water washing liquid is milky yellow. Continue to use anhydrous ethanol, the former is impregnated at a volume ratio of 1:7, 1:5, and 1:20, and the latter is impregnated at a volume ratio of 1:7, 1:5, and 1:10, each impregnation time is 30min, and the impregnation liquid is finally light yellow and transparent. Finally, the sample is naturally air-dried for 24h, placed in an oven (model DHG-9030A, manufacturer) at 105℃ for 4h, cooled, and white nano calcium carbonate is obtained. The final sample whiteness is 68.4 and 70.0 respectively measured by a whiteness meter, which are 78.4% and 80.2% of the standard whiteness respectively, which are 12% and 10.2% lower than the whiteness of the one-step burning whitening method. The bleaching method has the disadvantages of corrosive bleaching agents, high equipment requirements, and high bleaching agent costs. The bleaching process is affected by pH, material slurry mass fraction, temperature, bleaching agent dosage, and bleaching time, and is prone to secondary wastewater problems.

[0146] Performance test case

[0147] 1. Characterization methods

[0148] SEM (ZEISS GeminiSEM 300, Germany) was used to characterize the morphology of white nano-calcium carbonate prepared from biogas slurry and commercially available nano-calcium carbonate. A particle size distribution analyzer (Mastersizer 2000, Malvern, UK) was used to measure the particle size distribution of white nano-calcium carbonate and commercially available nano-calcium carbonate. X-ray diffractometer (XRD, Japan Rigaku Ultima IV) and X-ray fluorescence spectrometer (XRF, Japan SHIMADZU XRF-1800) were used to analyze the physical phase and elemental composition of white nano-calcium carbonate.

[0149] 2. Results

[0150] 2.1 Morphological characteristics

[0151] Figure 3a is the SEM morphology of a white nano-calcium carbonate sample carbonized at 700℃ for 2h under air fluidization at 10,000 times. It is spindle-shaped, cone-shaped, rod-shaped, and needle-shaped, with an uneven surface and good dispersion. This is because the carbon-containing organic matter coating the calcium carbonate volatilizes at 700℃, and the gas release process is conducive to the dispersion of calcium carbonate. Under a magnification of 50,000 times, the sample is interwoven with rods and spindles, presenting a dendritic shape, with many fine particles growing on the surface, and the surface is rough, belonging to the aragonite type ( Figure 3 b). Figure 3 c and Figure 3 d is the morphology of commercially available nano calcium carbonate under 10,000 times and 50,000 times microscopes. The particle size is small and it is a spherical aggregate, belonging to the vaterite type. Its dispersibility is not very good. From the SEM morphology analysis, it can be seen that the particle size of the white nano calcium carbonate prepared from biogas slurry is larger than that of commercially available nano calcium carbonate. It is necessary to further control the reaction conditions to enhance its dispersibility and reduce the particle size.

[0152] 2.2 Particle size distribution

[0153] The particle size distribution of white nano calcium carbonate prepared from biogas slurry was analyzed. Figure 4 .from Figure 4 It can be seen that the average particle size of white nano calcium carbonate within 10% is 1.081μm, the average particle size of white nano calcium carbonate within 50% is 6.606μm, and the average particle size of white nano calcium carbonate within 90% is 13.968μm. The average particle sizes of commercially available nano calcium carbonate within 10%, 50%, and 90% are 4.748μm, 10.260μm, and 18.632μm, respectively. Figure 4 ). From the perspective of particle size distribution, it can be seen that the particle size of white nano calcium carbonate prepared from biogas slurry is smaller than that of commercially available nano calcium carbonate.

[0154] 2.3 Crystal structure and composition

[0155] Figure 5It is the XRD diffraction peak of white nano calcium carbonate. Diffraction peaks appear at 2θ=23.0, 29.4, 36.0, 39.4, 43.1, 47.5, 48.5, 56.4, and 57.5°, corresponding to (012), (104), (110), (113), (202), (018), (116), (211), and (122) crystal planes, respectively, indicating that the crystal form of calcium carbonate is calcite. Calcite calcium carbonate is thermodynamically the most stable than aragonite and vaterite calcium carbonate. Although the morphology of nano calcium carbonate is spindle, rod, and needle, the crystal form is still calcite, indicating that the humic acid-based nano calcium carbonate produced by the synchronous double decomposition and coating reaction of biogas slurry is subjected to high-temperature fluidization at 700°C, the carbon-containing organic matter is volatilized, and the gas release dispersion is beneficial to the dispersion of calcium carbonate, and the crystal form does not change. The XRF elemental components of white nano-calcium carbonate with a proportion greater than 10% are classified, as shown in Table 1. The results show that Ca, O, and C are the main elemental components of white nano-calcium carbonate, indicating that at 700°C carbonization, the carbon-containing organic matter coated with nano-calcium carbonate volatilizes into gas and releases, which not only has a dispersing effect, but also burns the nano-calcium carbonate white.

[0156] Table 1 Elemental analysis results of white nano calcium carbonate

[0157]

[0158] SEM test method: Take a trace amount of nano-calcium carbonate sample and stick it directly on the conductive glue, and use Quorum SC7620 sputtering coater to spray gold for 45s (the specific gold spraying time is determined according to the sample / test requirements), and the gold spraying current is 10mA; then use ZEISSGeminiSEM 300 scanning electron microscope to take pictures of sample morphology, energy spectrum mapping and other tests. The acceleration voltage is 3kV when taking morphology, and the acceleration voltage is 15kV when taking energy spectrum mapping. The detector is SE2 secondary electron detector.

[0159] Particle size distribution test method: Use a particle size distribution analyzer (Mastersizer 2000, Malvern, UK), and fully mix the sample nano calcium carbonate; turn on the instrument and the particle size measurement software, turn on the accessory switch → turn on the optical component switch → turn on the computer, double-click, the instrument needs to be preheated for 15 to 30 minutes; select measure-manual → click Start test background software will automatically perform electronic background, optical background measurement and light Mastersizer 2000 icon, start the software, when the light energy trend is decreasing and the maximum should be less than 80, the last intensity = 80% or so, then proceed to the next step; click Next → Add sample to proceed, when the Obscuration shading is within the set range (green) condition, proceed to the next step; click Start → Test sample, the measurement results are saved in Records.

[0160] XRD test method: X-ray diffraction analysis of the sample was carried out on an X-ray diffractometer (Rigaku Ultima IV), with CuKα as the radiation source wavelength of 0.15418nm, the test range of 10° to 90°, the scanning speed of 0.02° / s, the tube voltage of 40kV and the current of 40mA.

[0161] XRF test method: On the X-ray fluorescence spectrometer (SHIMADZU XRF-1800), first turn on the external cooling water, then turn on the instrument power, the "RUN" indicator light on the host panel is on, turn on the PC power, start the Windows operating system, start the PC-XRF software, click Analysis, click Sample Registration, select Analysis, and perform quantitative analysis of the elemental composition of the nano calcium carbonate powder sample. The results are shown in Table 2.

[0162] Table 2 Characterization parameters

[0163]

[0164]

[0165] 3D Structure:

[0166] Conductive nano calcium carbonate: needle-shaped, rod-shaped, spindle-shaped, calcite-type crystal

[0167] Whiteness:

[0168] Nano calcium carbonate: The whiteness is 78.8, which is 90.4% of the standard whiteness (87.2), that is, when the whiteness value is full of 100, the whiteness of the product reaches 90.4.

[0169] In the description of the present application, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0170] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A method for preparing white nano calcium carbonate, It is characterized in that The following steps are involved: S1, separating the biogas slurry into solid and liquid, and collecting the separated liquid; S2, determining the alkalinity molar concentration of the biogas slurry water separation liquid in step S1, and determining the pH of the separation liquid; S3, the theoretical dosage of CaO calculated according to the alkalinity molar concentration of the step; S4, adding CaO according to the theoretical dosage of CaO to the biogas slurry water separation liquid in step S1, stirring until floccules are precipitated, and preparing a humic acid-based nano-calcium carbonate crude extract; S5, centrifuging the humic acid-based nano-calcium carbonate crude extract, collecting the precipitate, drying it, and carbonizing it at 700-825° C. for 2-4 hours in air or oxygen-enriched fluidized state to obtain the white nano-calcium carbonate; Step S2 specifically comprises: determining the alkalinity molar concentration of the biogas slurry water separation liquid in step S1 according to equations (1) and (2); (1) (2) in, Indicates the molar concentration of alkalinity of biogas slurry, mol / L; Indicates the molar concentration of a known acid, mol / L; represents the titration volume of the acid, L; Indicates the volume of the biogas slurry sample, L; Step S3 specifically comprises: according to the molar concentration of alkalinity of the biogas slurry in step S2, according to the double decomposition reaction formula (3), (4), and the formula (5) to calculate the theoretical dosage of CaO; wherein the dosage of CaO is such that the pH of the biogas slurry reaction is maintained in the range of 8.70 to 8.99; When Ca(OH) 2 insufficient: (3) When Ca(OH) 2 Adequate amount: (4) (5) (6) in, Indicates the molar concentration of CaO added, mol / L; represents the molar mass concentration of CaO, 56 g / mol; is the biogas slurry reaction volume, L; Indicates the theoretical addition mass of CaO, g; In reaction equations (3) and (4), Ca(OH) 2 / NH 4 HCO 3 The molar ratio is controlled at 0.5~1.

2. The preparation method according to claim 1, It is characterized in that The method further comprises step S6, wherein step S6 comprises the following steps: S61, centrifuge the humic acid-based nano-calcium carbonate crude extract of step S4, collect the supernatant into a dry container, measure the pH of the supernatant, and titrate the alkalinity of the biogas slurry with an acid solution according to formula (8) and formula (9). When the methyl orange indicator changes from orange to orange, stop the titration and record the titrated acid pH. + Volume △V, calculated carbonate CO 3 2- The molar concentration of S62. According to reaction formula (10) and reaction formula (11), calculate the amount of CaCl to be added. 2 The theoretical molar concentration value of S63. According to reaction formula (12), calculate CaCl 2 Theoretical dosage; add CaCl to the supernatant 2 , the pH value is controlled within the range of 7.0-7.5 at the end of the reaction; according to reaction formula (13), the NaOH solution is continued to be used for adjustment, the pH value rises to 8.3-8.5, the addition of the NaOH solution is stopped, the mixture is stirred for 10-20 minutes, and the mixture is allowed to stand for 10-20 minutes until a flocculent precipitate appears. The precipitate is collected, dried, and carbonized at 700-825°C for 2-4 hours in air or oxygen-enriched fluidized state to obtain the white nano calcium carbonate; (8) (9) (10) (11) (12) (13) Among them, represents the molar concentration of carbonate, mol / L; represents the molar concentration of the known acid, mol / L; represents the titration volume of the acid, L; represents the volume of the centrifuged collected liquid taken, L; represents the molar concentration of calcium chloride, mol / L; represents the molar mass concentration of calcium chloride, 111 g / mol; represents the total volume of the centrifuged collected supernatant, L; represents the theoretical k = 1 dosing mass of calcium chloride or the actual dosing mass when 0.5 < k < 1, g.

3. The preparation method according to claim 1, It is characterized in that In step S5, the drying conditions are: 100-140° C. oven drying for 8-12 hours.

4. The preparation method according to claim 1, It is characterized in that The biogas slurry water is the biogas slurry water from the anaerobic fermentation tank of Miaoji Biogas Station in Funan County, Anhui Province.

5. The preparation method according to claim 1, It is characterized in that In step S1, the solid-liquid separation of the biogas slurry is performed by a screw stacking machine.