Alumina carrier and its forming method and application
By using microsphere expansion agent and extrusion molding technology in the alumina carrier, an alumina carrier with a bimodal pore structure is formed, which solves the problems of pore size and mechanical strength in the existing technology and realizes an efficient residual oil hydrogenation catalyst. performance.
Patent Information
- Application Number
- CN202210038225.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-13
AI Technical Summary
The existing alumina carrier cannot meet the demand for hundreds of nanometer-sized pores in the hydrogenation process of residual oil, resulting in blockage of the pores and a decrease in the mechanical strength of the catalyst. Traditional pore expansion methods have low efficiency and poor penetration.
Microsphere expansion agent is mixed with alumina dry glue powder, and the temperature and pressure are controlled through extrusion molding technology to form an alumina carrier with a bimodal pore structure, ensuring a high proportion of hundreds of nanometer pores and good penetration.
The high mechanical strength and long-life catalyst of the alumina carrier is achieved, which can effectively demetallize the catalyst and is suitable for heavy oil hydrogenation reaction.
Smart Images

Figure BDA0003468963570000031 
Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] The invention relates to an alumina carrier and a molding method and application thereof, and in particular to an alumina carrier suitable for a hydrogenation catalyst in the petrochemical industry and a molding method and application thereof. Background Art
[0002] In the oil refining industry, heavy oil, especially residual oil, contains a large amount of metals, such as Fe, Ca, Ni, V, Na, etc., among which metals are mainly concentrated in asphaltene and colloid. In the process of residual oil hydrogenation, since the downstream is a heavy oil catalytic cracking unit, there are strict metal content restrictions on the feed oil, so most of the metal impurities must be removed in the process of residual oil hydrogenation, and the asphaltene molecules containing metals can reach ten nanometers. Therefore, for the existing alumina carrier, its pores are mainly concentrated between 2 and 12nm. Therefore, the asphaltene molecules are severely controlled by internal diffusion and are easily concentrated on the outer surface of the catalyst to react, resulting in serious pore blockage, which in turn causes a rapid increase in pressure drop and affects the normal operation of the device. Therefore, the residual oil hydrogenation catalyst is required to have a large number of hundreds of nanometer-level pores suitable for the diffusion reaction of asphaltene molecules.
[0003] The existing macroporous alumina carrier cannot meet the requirement of directly generating pores at the hundred-nanometer level, so it is a good choice to expand the existing alumina carrier to form a pore size distribution with bimodal pores at the ten-nanometer level and the hundred-nanometer level. However, whether a physical pore expander or a chemical pore expander is used, the existing pore expansion means have problems such as low efficiency of the pore expander, the need for a higher proportion of pore expanders, poor penetration of super-large pores, and the formation of ink bottle-shaped pores, which leads to a decrease in the mechanical strength of the catalyst. For example, CN 102861615B discloses a method for preparing an alumina carrier, which uses pseudo-boehmite, an extrusion aid, a chemical pore expander, an ammonium salt, a physical pore expander carbon black powder, and water to mix and knead extruded strips, but the pores formed by thermal decomposition of the ammonium salt and the holes formed by ablation of carbon black have poor penetration and low mechanical strength, and the utilization efficiency of the pore expander is low. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides an alumina carrier and its forming method and application. The alumina carrier has a through bimodal pore structure adjustable within a certain range, has a high proportion of 100-nanometer pores, can meet the diffusion requirements of macromolecular substances, and has the characteristics of high demetallization activity and long catalyst life when applied to residual oil hydrogenation reaction.
[0005] The first aspect of the present invention provides an alumina carrier, which has a through bimodal pore structure, and the pore volume of the alumina carrier is 0.8-1.3 mL / g; the pore volume occupied by pores with a pore diameter of 1-15 nm is 40%-92% of the total pore volume; the pore volume occupied by pores with a pore diameter of 50-900 nm is 5%-56% of the total pore volume.
[0006] According to the present invention, preferably, the pore volume of the alumina carrier is 0.9 to 1.2 mL / g.
[0007] According to the present invention, preferably, in the alumina carrier, the pore volume of pores with a pore diameter of 1 to 15 nm accounts for 43% to 77% of the total pore volume; the pore volume of pores with a pore diameter of 50 to 900 nm accounts for 22% to 53% of the total pore volume.
[0008] According to the present invention, in the alumina carrier, the concentration of the macropore distribution with a pore diameter of 50 to 900 nm can be adjusted, for example, the macropore distribution is concentrated in 60 to 400 nm, for example, the macropore distribution is concentrated in 60 to 120 nm, 60 to 140 nm, 60 to 150 nm, 150 to 300 nm or 150 to 400 nm, etc.
[0009] According to the present invention, the specific surface area of the alumina carrier is 80 to 300 m 2 / g, preferably 100 to 180 m 2 / g.
[0010] According to the present invention, the mechanical strength of the alumina carrier is 10 to 30 N / mm, preferably 10 to 20 N / mm.
[0011] According to the present invention, the shape of the alumina carrier can be a conventional shape in the art, such as a columnar, spherical, ellipsoidal, cylindrical, bar, impeller, toothed ball, clover, four-leaf clover and other special shapes, and holes can be opened on it, and grooves can be provided on the outer surface.
[0012] The second aspect of the present invention provides a method for forming the above-mentioned alumina carrier, comprising the following steps:
[0013] (1) Mix the aluminum oxide dry glue powder and the microsphere expansion agent evenly;
[0014] (2) kneading and shaping the materials after mixing in step (1);
[0015] (3) drying and calcining the molded product obtained in step (2) to obtain an alumina carrier;
[0016] The microsphere expansion agent in step (1) has a core-shell structure, wherein the outer shell is a thermoplastic acrylic polymer and the inner core is a hydrocarbon.
[0017] According to the present invention, the microsphere expansion agent in step (1) is a high temperature type. The shell temperature limit of the microsphere expansion agent in step (1) is 155°C to 210°C, preferably 160 to 185°C; the initial volatilization temperature of the core hydrocarbon is 110 to 145°C, preferably 120 to 135°C. The volume fraction of the core hydrocarbon volume to the shell volume is 0.0001% to 0.1%, preferably 0.0002% to 0.001%.
[0018] According to the present invention, the particle size of the microsphere expansion agent in step (1) is 1 μm to 100 μm, preferably 5 μm to 50 μm.
[0019] According to the present invention, the microsphere expansion agent in step (1) can be a commercial product or prepared according to the prior art. The commercial product can be at least one of Clocell high temperature foaming microspheres of POLYCHEM Company of the United States and Expancel DU series high temperature foaming microspheres of Nouryon Company of Switzerland. For example, the product models of Clocell high temperature foaming microspheres of POLYCHEM Company of the United States are 186DU20, 180DU25, 186DU35, 186DU45, and for another example, the product models of Expancel DU series high temperature foaming microspheres of Nouryon Company of Switzerland are 920DU20, 920DU40, 920DU80, 920DU120, etc.
[0020] According to the present invention, preferably, the properties of the microsphere expansion agent in step (1) have at least one of A to D:
[0021] serial number Particle size / μm Core initial volatile temperature / ℃ Shell temperature limit value / ℃ A 15~25 130~140 180~190 B 20~39 120~129 175~185 C 40~50 120~129 175~185 D 40~50 110~119 165~175
[0022] According to the present invention, preferably, the microsphere expansion agent in step (1) has at least one of the properties of E to H:
[0023]
[0024]
[0025] According to the present invention, the weight of the microsphere expansion agent added in step (1) is 2% to 30% of the weight of the alumina dry rubber powder, preferably 3% to 15%.
[0026] According to the present invention, the alumina dry rubber powder in step (1) is macroporous aluminum hydroxide.
[0027] According to the present invention, water, preferably deionized water, needs to be added in step (1); the amount of water added is 70% to 160% of the weight of the aluminum oxide dry rubber powder, preferably 110% to 130%. Water is added together with other raw materials in step (1).
[0028] According to the present invention, an extrusion aid can be added in step (1), and the extrusion aid is one or more of sesbania powder, cellulose, polyvinyl alcohol, polyacrylamide, methyl cellulose, and hydroxypropyl methyl cellulose; the amount of the extrusion aid added is 1% to 5% by weight of the alumina dry rubber powder, preferably 2% to 4%. The extrusion aid is added together with other raw materials in step (1).
[0029] According to the present invention, a peptizing agent may be added in step (1), wherein the peptizing agent is one or more of nitric acid, citric acid, sulfuric acid, acetic acid, and hydrochloric acid, and the amount added is 1% to 5% by weight of the alumina dry glue powder, preferably 2% to 3%. The peptizing agent is added together with the other raw materials in step (1).
[0030] According to the present invention, the molding process in step (2) should be controlled at a temperature 10°C to 50°C higher than the initial volatilization temperature of the microsphere expansion agent core in step (1), preferably 20°C to 40°C.
[0031] According to the present invention, the molding process in step (2) should be controlled at a temperature higher than the shell temperature limit of the microsphere expansion agent in step (1) by 5°C to 40°C, preferably 5°C to 25°C.
[0032] According to the present invention, the molding in step (2) can be extrusion molding; the molding process should be carried out in a high temperature resistant molding device capable of measuring the temperature, cooling and heating the material. The high temperature resistant temperature range of the molding device is 100°C to 350°C, preferably 120°C to 300°C. The molding device is an extruder; the thickness of the orifice plate of the extruder is a conventional thickness, such as 0.1 to 0.5 cm.
[0033] According to the present invention, preferably, the pressure during the molding process in step (2) should be controlled to be 100 kg / cm 2 ~180kg / cm 2 .
[0034] According to the present invention, the drying in step (3) is performed at 50-150°C for 1h-5h; the calcination is performed at 500-1000°C for 2h-5h, preferably 800-1000°C.
[0035] According to the present invention, a third aspect of the present invention provides use of the above-mentioned alumina carrier or the alumina carrier prepared by the above-mentioned method in a hydrogenation catalyst.
[0036] According to the present invention, when used as a hydrogenation catalyst, it can be obtained by using a common method in the art, that is, using a carrier to load an active metal component. The active metal is a Group VIB and / or Group VIII metal, the Group VIB metal is preferably molybdenum and / or tungsten, and the Group VIII metal is preferably cobalt and / or nickel. Based on the mass of the carrier, the content of the Group VIB metal oxide is 1% to 20%, and the content of the Group VIII metal oxide is 0.1% to 8%.
[0037] According to the present invention, the raw material for hydrotreatment is residual oil, and the properties of the residual oil are as follows: the Ni+V content is 20 to 150 ppm. The content is mass content.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] (1) In the present invention, the alumina carrier has a bimodal pore structure with good permeability, and the pore volume of the alumina carrier is 0.8-1.3 mL / g; the pore volume occupied by pores with a pore diameter of 1-15 nm is 40%-92% of the total pore volume; the pore volume occupied by pores with a pore diameter of 50-900 nm is 5%-56% of the total pore volume. The alumina carrier of the present invention has a bimodal pore structure with good permeability that is adjustable within a certain range, has a high proportion of 100-nanometer pores, can meet the diffusion requirements of macromolecular substances, and is used in residual oil hydrogenation reactions with the characteristics of high demetallization activity and long catalyst life.
[0040] (2) In the present invention, in the molding method of the alumina carrier, a small amount of microsphere expansion agent is added to the alumina dry rubber powder, and the microsphere expansion agent is controlled to perform moderate and controllable pore expansion by controlling the appropriate temperature during extrusion molding through the shape limitation of the extruder and the extrusion pressure, thereby obtaining an alumina carrier having both an adjustable through bimodal pore distribution and high mechanical strength. The method of the present invention avoids the problems of using a traditional pore expansion agent to expand the pores to obtain pores of the order of hundreds of nanometers, such as large amount of pore expansion agent, poor mechanical strength, poor penetration of super-large pores, and formation of ink bottle-shaped pores. Alumina expanded with a microsphere expansion agent is particularly suitable for use as a heavy oil hydrogenation catalyst carrier. The hydrogenation catalyst obtained by loading the active metal on the alumina carrier has the characteristics of high demetallization activity and long catalyst life when used in residual oil hydrogenation reactions.
[0041] (3) In the present invention, the alumina carrier is suitable for use as a heavy oil hydrogenation catalyst carrier. The hydrogenation catalyst obtained by loading the active metal component on the alumina carrier has the characteristics of high demetallization activity and long catalyst life when used in residual oil hydrogenation reaction. DETAILED DESCRIPTION
[0042] The effects and results of the method of the present invention are further described below with reference to the embodiments, but are not limited to the following embodiments.
[0043] In the present invention, the pore volume and pore distribution are measured by mercury intrusion method; the mechanical strength is measured by a particle strength tester; and the specific surface area is measured by BET method.
[0044] The alumina dry glue powder used in the examples and comparative examples of the present invention is macroporous aluminum hydroxide, and its specific surface area is 245m 2 / g, pore volume is 0.89mL / g, and pore diameter is 12.5nm; pore distribution: pore diameters of 1-15nm account for 96.7%, and 16nm-900nm account for 3.3%.
[0045] In the present invention, the microsphere expansion agent of Example 4 is Clocell high-temperature foaming microspheres produced by POLYCHEM Company of the United States, model 180DU45, the particle size of this batch is 45 μm, the initial volatilization temperature of the core hydrocarbon is 125°C, and the temperature resistance limit value of the outer shell thermoplastic acrylate polymer is 180°C.
[0046] In the present invention, the microsphere expansion agent of Examples 1, 2, 3, 5, and 6 is Expancel DU series high-temperature foaming microspheres of Nouryon Company of Switzerland, model 920DU20, the average particle size of this batch is 7 μm, the initial volatilization temperature of the inner core hydrocarbon is 130°C, and the temperature resistance limit value of the outer shell thermoplastic acrylate polymer is 170°C.
[0047] In the present invention, the pressure of the molding process in each example is controlled to be 140 kg / cm 2 .
[0048] In the present invention, the Ni removal rate / % and V removal rate / % of the embodiments and comparative examples are:
[0049] Ni removal rate / %=1-(Ni mass content in produced oil / Ni mass content in raw oil)×100%;
[0050] V removal rate / %=1-(V mass content in the produced oil / V mass content in the raw oil)×100%.
[0051] In each example of the present invention, the thickness of the perforated plate of the extruder is 0.5 cm.
[0052] Example 1
[0053] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder that can measure the temperature, cool and heat the materials for extrusion molding. The temperature of the molding process is controlled to be 170°C to obtain alumina wet strips after pore expansion. Dry in an oven at 110°C at normal pressure for 2h, and after drying, calcine at 850°C for 3h to obtain an alumina carrier.
[0054] The pore volume of the alumina carrier is 0.95 mL / g, and the pore volume of pores with a pore diameter of 1 to 15 nm accounts for 84.9% of the total pore volume. The pores with a pore diameter greater than 15 nm are mainly distributed in the range of 60 nm to 150 nm, and the pore volume of pores with a pore diameter of 60 nm to 150 nm accounts for 13.1% of the total pore volume. The mechanical strength of the alumina carrier is 18 N / mm, and the specific surface area is 130 m 2 / g.
[0055] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0056] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties of the residual oil hydrogenation reaction are shown in Table 1. The hydrogenation reaction conditions are: temperature 380°C, pressure 15MPa, liquid hourly volume space velocity 1h -1 , hydrogen to oil volume ratio 760. The hydrogenation effect is shown in Table 2.
[0057] Example 2
[0058] Weigh 15g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling and heating the material for extrusion molding. The temperature of the molding process is controlled to be 170°C to obtain alumina wet strips after pore expansion. Dry in an oven at 110°C at normal pressure for 2h, and after drying, calcine at 850°C for 3h to obtain an alumina carrier.
[0059] The pore volume of the alumina carrier is 1.19 mL / g, and the pore volume of pores with a pore diameter of 1 to 15 nm accounts for 44.1% of the total pore volume. The pores with a pore diameter greater than 15 nm are mainly distributed in the range of 60 nm to 150 nm, and the pore volume of pores with a pore diameter of 60 nm to 150 nm accounts for 51.1% of the total pore volume. The mechanical strength of the carrier is 10 N / mm, and the specific surface area is 105 m 2 / g.
[0060] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% tungsten oxide and 2wt% cobalt oxide based on the mass of the carrier.
[0061] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0062] Example 3
[0063] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling and heating the material for extrusion molding. The temperature of the molding process is controlled to be 185°C to obtain alumina wet strips after pore expansion. Dry in an oven at 110°C at normal pressure for 2h, and after drying, calcine at 850°C for 3h to obtain an alumina carrier.
[0064] The pore volume of the alumina carrier is 0.93 mL / g, and the pore volume of pores with a pore diameter of 1 to 15 nm accounts for 87.6% of the total pore volume. The pores with a pore diameter greater than 15 nm are mainly distributed in the range of 60 nm to 120 nm, and the pore volume of pores of 60 nm to 120 nm accounts for 11.9% of the total pore volume. The mechanical strength of the carrier is 19 N / mm, and the specific surface area is 135 m 2 / g.
[0065] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% tungsten oxide and 2wt% nickel oxide based on the mass of the carrier.
[0066] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0067] Example 4
[0068] Weigh 3g of 180DU45 microspheres, the volume fraction of the hydrocarbon in the core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.0002%. Mix the microspheres with 100g of alumina dry powder, 120g of deionized water, 2g of sesbania powder, and 2ml of nitric acid, and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling, and heating the materials for extrusion molding. The temperature of the molding process is controlled at 185°C, and the alumina wet strips after pore expansion are dried in an oven at 110°C at normal pressure for 2h. After drying, they are calcined at 850°C for 3h to obtain the alumina carrier.
[0069] The pore volume of the alumina carrier is 0.94 mL / g, pores with a pore diameter of 1 to 15 nm account for 86.7%, pores with a pore diameter greater than 15 nm are mainly distributed in the range of 60 nm to 140 nm, and the pore volume of pores with a pore diameter of 60 nm to 140 nm accounts for 11.2% of the total pore volume. The mechanical strength of the carrier is 18 N / mm, and the specific surface area is 138 m 2 / g.
[0070] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% of molybdenum oxide and 2wt% of cobalt oxide based on the mass of the carrier.
[0071] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0072] Example 5
[0073] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the thermoplastic acrylate polymer spherical shell is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling and heating the materials for extrusion molding. The temperature of the molding process is controlled at 160°C, and the alumina wet strips after pore expansion are dried in an oven at 110°C at normal pressure for 2h. After drying, they are calcined at 850°C for 3h to obtain the alumina carrier.
[0074] The pore volume of the alumina carrier is 0.98 mL / g, pores with a pore diameter of 1 to 15 nm account for 68.8%, pores with a pore diameter greater than 15 nm are mainly distributed in the range of 150 nm to 400 nm, and the pore volume of pores with a pore diameter of 150 nm to 400 nm accounts for 24.3% of the total pore volume. The mechanical strength of the carrier is 14 N / mm, and the specific surface area is 120 m 2 / g.
[0075] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0076] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0077] Example 6
[0078] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling and heating the materials for extrusion molding. The temperature of the molding process is controlled at 195°C, and the alumina wet strips after pore expansion are dried in an oven at 110°C at normal pressure for 2h. After drying, they are calcined at 850°C for 3h to obtain the alumina carrier.
[0079] The pore volume of the alumina carrier is 0.97 mL / g, pores with a pore diameter of 1 to 15 nm account for 70.9%, pores with a pore diameter greater than 15 nm are mainly distributed in the range of 150 nm to 300 nm, and the pore volume of pores with a pore diameter of 150 nm to 300 nm accounts for 23.1% of the total pore volume. The mechanical strength of the carrier is 15 N / mm, and the specific surface area is 122 m 2 / g.
[0080] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0081] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0082] Comparative Example 1
[0083] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder that can measure the temperature, cool and heat the materials for extrusion molding. The temperature of the molding process is controlled to be 100°C to obtain the alumina wet strips after pore expansion. Dry in an oven at 110°C at normal pressure for 2h, and after drying, calcine at 850°C for 3h to obtain the alumina carrier.
[0084] The pore volume of the alumina carrier is 0.90mL / g, pores with a pore diameter of 1 to 15nm account for 93.9%, pores with a pore diameter greater than 15nm account for 6.1% of the total pore volume, pores with a pore diameter greater than 15nm are mainly distributed in the range of 1μm to 10μm, and the pore volume of 1μm to 10μm accounts for 2.8% of the total pore volume. The mechanical strength of the carrier is 21N / mm, and the specific surface area is 128m 2 / g.
[0085] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0086] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0087] Comparative Example 2
[0088] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 0.001%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature extruder capable of measuring, cooling and heating the materials for extrusion molding. The temperature of the molding process is controlled to be 225°C to obtain the alumina wet strips after pore expansion. Dry them in an oven at 110°C at normal pressure for 2h, and after drying, calcine them at 850°C for 3h to obtain the alumina carrier.
[0089] The pore volume of the alumina carrier is 0.90mL / g, pores with a pore diameter of 1 to 15nm account for 93.5%, pores with a pore diameter greater than 15nm account for 6.5% of the total pore volume, pores with a pore diameter greater than 15nm are mainly distributed in the range of 1μm to 10μm, and the pore volume of 1μm to 10μm accounts for 2.6% of the total pore volume. The mechanical strength of the carrier is 21N / mm, and the specific surface area is 129m 2 / g.
[0090] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0091] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0092] Comparative Example 3
[0093] Weigh 3g of 920DU20 microspheres, the volume fraction of the hydrocarbon core to the volume fraction of the spherical shell of the thermoplastic acrylate polymer is 10%. Mix the microspheres with 100g of alumina dry powder and 120g of deionized water and knead them thoroughly. Put the kneaded materials into a high-temperature resistant extruder that can measure, cool and heat the material for extrusion molding. The temperature of the molding process is controlled at 170°C to obtain wet alumina strips with expanded holes. Dry in an oven at 110°C at normal pressure for 2h. After drying, calcine at 850°C for 3h to obtain an alumina carrier. The alumina carrier obtained by extrusion has a fried strip phenomenon, an irregular shape, and visible millimeter holes on the surface. The mechanical strength of the carrier is 5N / mm. The specific surface area is 99m 2 / g.
[0094] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0095] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0096] Comparative Example 4
[0097] Weigh 3g of acrylonitrile-methacrylonitrile copolymer, 100g of alumina dry rubber powder and 120g of deionized water, mix and knead thoroughly, and put the kneaded materials into a high-temperature resistant extruder capable of measuring, cooling and heating the materials for extrusion molding. The temperature of the molding process is controlled at 170°C to obtain alumina wet strips after pore expansion. Dry in an oven at 110°C at normal pressure for 2h, and after drying, calcine at 850°C for 3h to obtain an alumina carrier.
[0098] The pore volume of the alumina carrier is 0.90 mL / g, pores with a pore diameter of 1 to 15 nm account for 96.1%, pores with a pore diameter greater than 15 nm are mainly distributed in the range of 16 nm to 25 nm, and the pore volume of pores with a pore diameter of 16 nm to 25 nm accounts for 2.1% of the total pore volume. The mechanical strength of the alumina carrier is 24 N / mm. The specific surface area is 131 m 2 / g.
[0099] The alumina carrier is impregnated with an impregnation liquid containing active metals to obtain a hydrogenation catalyst. The hydrogenation catalyst contains 5wt% molybdenum oxide and 2wt% nickel oxide based on the mass of the carrier.
[0100] The above hydrogenation catalyst was applied to the residual oil hydrogenation reaction. The raw oil properties and hydrogenation reaction conditions of the residual oil hydrogenation reaction were the same as those in Example 1. The hydrogenation effect is shown in Table 2.
[0101] Table 1 Raw oil properties
[0102] nature Raw oil-sand residue <![CDATA[Density (20 °C) / g·cm -3 > 0.9718 S / wt% 3.3 Ni / ppm 22.4 V / ppm 73.7
[0103] Table 2 Hydrogenation results obtained in each case
[0104] Ni removal rate / % V removal rate / % Example 1 54 80 Example 2 62 91 Example 3 55 83 Example 4 56 80 Example 5 60 88 Example 6 58 88 Comparative Example 1 40 68 Comparative Example 2 42 65 Comparative Example 3 38 70 Comparative Example 4 41 61
[0105] The above describes the specific implementation of the present invention in detail, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the various technical features being combined in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. An application of an alumina carrier in a hydrogenation catalyst, which is applied to the hydrodemetallization reaction of residual oil; The alumina carrier has a through bimodal pore structure, and the pore volume of the alumina carrier is 0.8-1.3 mL / g; the pore volume of pores with a pore diameter of 1-15 nm accounts for 40%-92% of the total pore volume; the pore volume of pores with a pore diameter of 50-900 nm accounts for 5%-56% of the total pore volume; The molding method of the alumina carrier comprises the following steps: (1) Mix the alumina dry glue powder and microsphere expansion agent evenly; (2) kneading and molding the mixed materials in step (1); (3) drying and calcining the molded product obtained in step (2) to obtain an alumina carrier; The microsphere expansion agent in step (1) has a core-shell structure, wherein the outer shell is a thermoplastic acrylic polymer and the inner core is a hydrocarbon; The volume fraction of the inner core hydrocarbon volume to the outer shell volume is 0.0001% to 0.1%; The molding process in step (2) should be controlled at a temperature higher than the initial volatilization temperature of the microsphere expansion agent core in step (1) by 10°C to 50°C, or the molding process in step (2) should be controlled at a temperature higher than the temperature limit of the shell of the microsphere expansion agent in step (1) by 5°C to 40°C; The weight of the microsphere expansion agent added in step (1) is 2% to 30% of the weight of the alumina dry glue powder.
2. The application according to claim 1, characterized in that: The volume fraction of the inner core hydrocarbon volume to the outer shell volume is 0.0002%~0.001%.
3. The application according to claim 1, characterized in that: The outer shell temperature limit of the microsphere expansion agent in step (1) is 155°C to 210°C; the initial volatilization temperature of the hydrocarbon in the inner core is 110°C to 145°C.
4. The use according to claim 3, characterized in that: The outer shell temperature limit of the microsphere expansion agent in step (1) is 160-185°C; the initial volatilization temperature of the hydrocarbon in the inner core is 120-135°C.
5. The use according to claim 1, characterized in that: The microsphere expansion agent in step (1) has at least one of properties A to D: 。 6. The use according to claim 1, characterized in that: The microsphere expansion agent in step (1) has at least one of the properties of E to H: 。 7. The use according to claim 1, characterized in that: The weight of the microsphere expansion agent added in step (1) is 3% to 15% of the weight of the alumina dry glue powder.
8. The use according to claim 1, characterized in that: The particle size of the microsphere expansion agent in step (1) is 1 μm to 100 μm.
9. The use according to claim 8, characterized in that: The particle size of the microsphere expansion agent in step (1) is 5 μm to 50 μm.
10. The use according to claim 1, characterized in that: The molding process in step (2) should be controlled at a temperature 20°C to 40°C higher than the initial volatilization temperature of the microsphere expansion agent core in step (1); Alternatively, the molding process in step (2) should be controlled at a temperature higher than the shell temperature limit of the microsphere expansion agent in step (1) by 5°C to 25°C.
11. The use according to claim 1, characterized in that: The drying in step (3) is performed at 50-150°C for 1h-5h; and the calcination is performed at 500-1000°C for 2h-5h.
12. The use according to claim 11, characterized in that: The calcination temperature in step (3) is 800-1000°C.
13. The use according to claim 1, characterized in that: The pore volume of the alumina carrier is 0.9-1.2 mL / g; the pore volume of pores with a pore diameter of 1-15 nm accounts for 43%-77% of the total pore volume; the pore volume of pores with a pore diameter of 50-900 nm accounts for 22%-53% of the total pore volume.
14. The use according to claim 1 or 13, characterized in that: The mechanical strength of the alumina carrier is 10-30 N / mm.
15. The use according to claim 14, characterized in that: The mechanical strength of the alumina carrier is 10-20 N / mm.