Welding structure of tab, battery and tab welding process
By welding the bent parts on the pins in the battery ear welding structure and limiting the pre-soldering area, the problems of low battery energy density and inconsistent welding are solved, and the welding efficiency and battery performance are improved.
Patent Information
- Application Number
- CN202310537428.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing battery electrode electrode welding structures lead to problems such as low energy density, inconsistent welding and low efficiency, especially due to the spatial redundancy in the connection direction of the electrode electrode and the pole column and the difficulty of adjusting the welding head.
Design an extreme ear welding structure in which the bent part is welded to the pin, and the area of the pre-soldered printing surface is fixed by defining the length and width (4mm≤a1≤8mm, 37mm≤b1≤41mm) to improve welding efficiency and Consistency and optimize welding quality through moving and swinging welding trajectories.
It improves the energy density of the battery and the consistency and efficiency of the extreme ear welding, avoids the risks of welding short circuits and overheating, optimizes the melting depth and melting width of the welding surface, and improves the charging performance of the battery.
Smart Images

Figure CN118943672A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a tab welding structure, a battery, and a tab welding process. Background Art
[0002] With the development of battery technology, batteries have been widely used in different fields such as smart phones, power tools and new energy vehicles.
[0003] The battery includes an outer shell, a battery cell arranged in the outer shell, and a top cover closed on the opening of the outer shell. There are two structures for electrically connecting the pole tabs on the battery cell with the pole posts on the top cover. One is that the pole tabs are connected to the pole posts through adapters. In this way, since the pole tabs and the pole posts have a large spatial redundancy in the connection direction, the energy density of the battery will be lower. In another way, the pole tabs are connected to the pole posts through pins. In this way, the welding head needs to be frequently adjusted according to the bending of the pole tabs so that the pole tabs are welded and fixed on the pins, which makes it difficult to ensure the consistency and efficiency of the pole tab welding. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a welding structure of a tab, a battery and a tab welding process, which can not only improve the energy density of the battery, but also improve the consistency and welding efficiency of the tab welding.
[0005] In order to solve the above technical problems, in a first aspect, the present invention provides a welding structure of a pole lug, wherein the welding structure of the pole lug comprises:
[0006] At least two cells;
[0007] At least two pole lugs, at least two of the pole lugs correspond to at least two of the battery cells one by one, each of the pole lugs comprises a connecting portion and a bending portion connected by bending, one end of the connecting portion away from the bending portion is connected to the end face of the corresponding battery cell, the bending portions of two adjacent pole lugs of at least two of the pole lugs extend toward each other in a direction parallel to a first direction, and an insertion gap is provided between the bending portions extending toward each other in two adjacent pole lugs and the end face of the battery cell, and the first direction is the direction of the thickness of the battery cell;
[0008] The pin is inserted in the insertion gap, and the bent portion is welded to the pin, the pre-welded surface of the bent portion of each of the tabs has a width a1 in the first direction and in a direction parallel to the end face of the battery cell, and a length b1 in the second direction, 4mm≤a1≤8mm, and 37mm≤b1≤41mm, and the second direction is parallel to the first direction and the end face of the battery cell.
[0009] By welding the bent portion to the pin, and the pin is located between the bent portion and the battery cell, the distance between the top cover and the battery cell can be reduced, thereby improving the energy density of the battery. In addition, by the width of the pre-welding surface of the bent portion in the first direction being a1, the length in the direction perpendicular to the first direction being b1, 4mm≤a1≤8mm, and 37mm≤b1≤41mm, the area of the pre-welding surface of the bent portion can be limited, thereby limiting the pre-welding range of the welding head. Therefore, when the bent portion of the pole ear is welded to the pin, it is only necessary to make the welding head weld the bent portion of the pole ear within the area of the pre-welding surface. On the one hand, there is no need to frequently adjust the welding head, thereby improving the efficiency of the pole ear welding. On the other hand, it can improve the consistency of the penetration depth and penetration width of the welding surface of the bent portion of the pole ear, thereby improving the consistency of the pole ear welding.
[0010] In addition, when the length b1 of the pre-weld printed surface is less than 37mm and the width a1 is less than 4mm, the area of the pre-weld printed surface will be too small, thereby affecting the welding effect between the bent portion of the pole ear and the pin. When the length b1 of the pre-weld printed surface is greater than 41mm and the width a1 is greater than 8mm, the length of the pole ear will be increased, making the pole ear too long, causing the bent portion to exceed the center of the end face of the battery cell, and thus easily causing a short circuit between the bent portions on opposite sides of the end face of the battery cell. Therefore, through comprehensive consideration, 4mm≤a1≤8mm, and 37mm≤b1≤41mm. In this way, it can avoid affecting the welding effect between the bent portion of the pole ear and the pin due to the small area of the pre-weld printed surface, and avoid a short circuit in the bent portion to affect the normal use of the battery.
[0011] In a possible implementation of the first aspect, the effective weld surface between the bent portion of one of the tabs and the pin is a2 wide in the first direction and b2 long in the second direction, 1.5mm≤a2≤3mm, and 33mm≤b2≤39mm, and the second direction is parallel to the first direction and the end face of the battery cell.
[0012] When a2 is less than 1.5mm and b2 is less than 33mm, the effective welding area between the bent portion of the pole ear and the pin will be smaller, thereby affecting the welding stability between the bent portion of the pole ear and the pin. In addition, when a2 is less than 1.5mm, since the welding width is too small, bubbles and slag residues are likely to appear during the welding process between the bent portion and the pin, resulting in too high protrusion of the welding surface, and then resulting in insufficient molten width and depth of the welding surface, which affects the welding effect between the bent portion and the pin. When a2 is greater than 3mm and b2 is greater than 39mm, since the effective welding area between the bent portion of the pole ear and the pin is larger, there is an area that exceeds the pre-weld printed surface of the bent portion of the pole ear. In this case, it will affect the welding effect between the bent portion of the pole ear and the pin, and the conduction capacity between the pole ear and the pin, thereby affecting the charging performance of the battery.
[0013] Based on this, through comprehensive consideration, 1.5mm≤a2≤3mm, and 33mm≤b2≤39mm, so that it can avoid affecting the welding stability between the bent part of the pole ear and the pin due to the small effective welding area between the bent part of the pole ear and the pin, and improve the melting depth and width of the welding surface, thereby improving the welding effect between the bent part and the pin, and also improve the conduction capacity between the pole ear and the pin, thereby improving the charging performance of the battery.
[0014] In a possible implementation manner of the first aspect, the pin is a copper pin, and the thickness of the copper pin is m1, 1.8 mm ≤ m1 ≤ 2.3 mm; or,
[0015] The pin is an aluminum pin, and the thickness of the aluminum pin is m2, 2.8mm≤m2≤3.3mm.
[0016] When the thickness of the copper pin is less than 1.8 mm, the structural strength of the copper pin is low, thereby affecting the welding effect between the copper pin and the bent portion. In addition, the thinner copper pin can also affect the current carrying capacity of the copper pin. When the thickness of the copper pin is greater than 2.3 mm, it is not conducive to the high energy density design of the battery. Therefore, the thickness of the copper pin is between 1.8 mm and 2.3 mm.
[0017] Similarly, when the thickness of the aluminum pin is less than 2.8mm, the structural strength of the aluminum pin is low, thereby affecting the welding effect between the aluminum pin and the bent portion. In addition, the thinner aluminum pin can also affect the current carrying capacity of the aluminum pin. When the thickness of the aluminum pin is greater than 3.3mm, it is not conducive to the high energy density design of the battery. Therefore, the thickness of the aluminum pin is between 2.8mm and 3.3mm.
[0018] In a second aspect, the present invention further provides a battery, comprising:
[0019] a housing, the interior of the housing being hollow and having an opening communicating with the interior of the housing;
[0020] The electrode tab welding structure described in the first aspect, wherein the battery cell in the electrode tab welding structure is arranged inside the shell, and the end surface of the battery cell is opposite to the side wall of the shell, and the side wall of the battery cell is opposite to the opening;
[0021] A top cover is installed on the opening, and the top cover includes a pole connected to the pin.
[0022] Since the end face of the battery cell is opposite to the side wall of the shell, the side wall of the battery cell is opposite to the opening, the pins extend toward the inside of the shell to be inserted into the insertion gap, and the pole is connected to the pins. Therefore, in the direction of the opening, the top cover is opposite to the side wall of the battery cell, and no space is reserved in this direction for the connection between the pole ear and the adapter sheet and the adapter sheet and the pole. It can be seen that space is saved in the direction of the opening, thereby improving the energy density of the battery. In addition, the pole ear can be electrically connected to the pole through the pins.
[0023] In addition, since the battery includes the welding structure of the electrode tab in the first aspect, the overall performance of the battery is improved.
[0024] In a third aspect, the present invention further provides a tab welding process, the welding process is used to weld the tab welding structure described in the first aspect, the process comprising:
[0025] Inserting the pin into the insertion gap;
[0026] The bent portion is welded to the pin using a moving and swinging welding track.
[0027] Therefore, by adding vibration to the moving welding trajectory, the bent portion and the pin can be welded at a faster speed, and the metallographic effect of the weld can be optimized, thereby achieving the purpose of improving the quality of laser welding by optimizing the welding trajectory.
[0028] In a possible implementation of the third aspect, the welding trajectory is one of a sine curve, a double helix curve, and a cross straight line.
[0029] Since the welding trajectory of the sine curve is a smooth arc transition at the bend, it can reduce welding spatter and optimize the appearance of the weld line. In addition, since there are more welding overlaps in the welding trajectory of the double helix curve, the welding depth can be increased, which can be applied to the welding of thicker materials. In addition, since the welding trajectory of the cross straight line has a better distribution uniformity, it can optimize the welding pool and reduce the porosity slag inside the welding pool.
[0030] In a possible implementation of the third aspect, the welding trajectory is any two of a sine curve, a double helical curve, and a cross straight line, or the welding trajectory includes a sine curve, a double helical curve, and a cross straight line.
[0031] Since the sinusoidal welding trajectory can reduce welding spatter and optimize the appearance of the weld line, the double helix curve welding trajectory can increase the welding depth and is used for welding thicker materials, the cross straight line welding trajectory can optimize the welding molten pool and reduce the porosity slag inside the welding molten pool, and the cross straight line welding trajectory can be used for primer, therefore, when any two welding trajectories of the sinusoidal curve, double helix curve, and cross straight line are combined, the effects of each welding trajectory can be superimposed, and the welding metallographic structure can be further optimized to avoid overheating of welding, thereby reducing the risk of thermal runaway during welding.
[0032] When the welding trajectory is a combination of a sine curve, a double helix curve and a cross straight line, it can add the effects of each welding trajectory while reducing welding protrusions, welding surface pores, metallographic bubbles and slag, thereby improving the fullness of the weld line and the welding metallography, making the welding metallography as free of bubbles and slag as possible.
[0033] In a possible implementation of the third aspect, before the bending portion is welded to the pin by using a moving and swinging welding track, the process includes:
[0034] Clamping and positioning the pin and the tab;
[0035] The bending portion is pre-welded by ultrasonic welding.
[0036] Thus, the welding head can be vibrated at a specific frequency and amplitude to pre-weld the bent portion of the pole ear, thereby welding the multi-layered bent portions into a whole, in preparation for the laser welding device to weld the bent portion to the pin.
[0037] In a possible implementation of the third aspect, the step of welding the bent portion to the pin by using a moving and swinging welding track includes:
[0038] The bent portion is welded to the pin by laser welding, and the width of the laser welding is greater than or equal to 2 mm.
[0039] When the width of the laser weld is less than 2mm, it is difficult to ensure the effective molten width of the bend welding surface. In other words, when the width of the laser weld is less than 2mm, due to the narrow effective molten width of the bend welding surface, bubbles and slag residues are easily generated on the bend welding surface during the laser welding process, which makes the welding surface convex, thus affecting the welding quality of the laser weld. Based on this, limiting the width of the laser weld to 2mm or more can ensure that the effective molten width of the bend welding surface is 1.5mm or more, so that the bubbles and slag residues on the welding surface can be reduced, thereby improving the welding quality of the laser weld.
[0040] In a possible implementation of the third aspect, the process further includes:
[0041] Before welding, the welding surfaces of the bent portion and the pin are both smooth surfaces.
[0042] Since the smooth surface can cause reflection of the laser beam, the risk of adverse effects such as welding penetration caused by laser welding on the welding surface can be reduced, thereby improving the welding effect between the bent portion and the pin.
[0043] Compared with the prior art, this application has at least the following beneficial effects:
[0044] In the present application, by welding the bent portion to the pin, and the pin is located between the bent portion and the battery cell, the distance between the top cover and the battery cell can be reduced, thereby improving the energy density of the battery. In addition, by the pre-welding surface of the bent portion having a width of a1 in the first direction and a length of b1 perpendicular to the first direction, 4mm≤a1≤8mm, and 37mm≤b1≤41mm, the area of the pre-welding surface of the bent portion can be limited, thereby limiting the pre-welding range of the welding head. Therefore, when the bent portion of the pole ear is welded to the pin, it is only necessary to allow the welding head to weld the bent portion of the pole ear within the area of the pre-welding surface. On the one hand, there is no need to frequently adjust the welding head, thereby improving the efficiency of the pole ear welding. On the other hand, it can improve the consistency of the penetration depth and penetration width of the welding surface of the bent portion of the pole ear, thereby improving the consistency of the pole ear welding.
[0045] In addition, by 4mm≤a1≤8mm and 37mm≤b1≤41mm, it is possible to avoid affecting the welding effect between the bent portion of the tab and the pin due to the small area of the pre-welding print surface, and to avoid short circuit in the bent portion to affect the normal use of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0047] Figure 1 A schematic structural diagram of a welding structure of a tab provided in an embodiment of the present invention;
[0048] Figure 2 A schematic diagram of the structure of the connection between the tab and the battery cell provided in an embodiment of the present invention;
[0049] Figure 3 A schematic diagram of the structure of the pre-weld printed surface on the tab provided by an embodiment of the present invention;
[0050] Figure 4 A schematic diagram of the structure of an effective welding surface on a tab provided by an embodiment of the present invention;
[0051] Figure 5 A schematic diagram of an exploded structure of a battery provided by an embodiment of the present invention;
[0052] Figure 6 A schematic diagram of a process flow of a tab welding process provided by an embodiment of the present invention;
[0053] Figure 7 One of the structural schematic diagrams of the laser welding device provided in an embodiment of the present invention;
[0054] Figure 8 A second structural schematic diagram of a laser welding device provided in an embodiment of the present invention;
[0055] Fig. 9 A schematic structural diagram of a sinusoidal welding trajectory provided by an embodiment of the present invention;
[0056] Fig.10 A schematic diagram of the structure of a double helix curve welding trajectory provided by an embodiment of the present invention;
[0057] Fig.11 A schematic diagram of the structure of the welding track of the intersecting straight lines provided in an embodiment of the present invention;
[0058] Fig.12 A schematic diagram of the structure of a welding trajectory of a combination of a sine curve and a double helical curve provided in an embodiment of the present invention;
[0059] Fig.13 A schematic diagram of the structure of a welding trajectory composed of a sine curve, a double helical curve and intersecting straight lines provided in an embodiment of the present invention;
[0060] Fig.14 A schematic structural diagram of an ultrasonic welding device provided in an embodiment of the present invention.
[0061] Description of reference numerals:
[0062] 100-welding structure of the pole ear; 110-battery core; 120-pole ear; 121-connecting portion; 122-bending portion; 123-insertion gap; 124-pre-welding surface; 125-effective welding surface; 130-pin;
[0063] 200 - battery; 220 - housing; 221 - opening; 230 - top cover; 231 - pole;
[0064] 300-laser welding device; 310-collimating mirror; 320-focusing mirror; 330-galvanometer mirror;
[0065] 400 - ultrasonic welding device; 410 - transducer; 420 - amplitude modulator; 430 - welding head. DETAILED DESCRIPTION
[0066] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0067] In the present invention, the directions or positional relationships indicated by the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "vertical", "horizontal", "lateral", "longitudinal" and the like are based on the directions or positional relationships shown in the drawings. These terms are mainly used to better describe the present invention and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific direction, or to be constructed and operated in a specific direction.
[0068] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those skilled in the art, the specific meanings of these terms in the present invention can be understood according to specific circumstances.
[0069] In addition, the terms "installed", "set", "provided with", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0070] In addition, the terms "first", "second", etc. are mainly used to distinguish different devices, elements or components (the specific types and structures may be the same or different), and are not used to indicate or imply the relative importance and quantity of the indicated devices, elements or components. Unless otherwise specified, "plurality" means two or more.
[0071] As described in the background technology of the present application, in the related technology, the battery includes a shell, a battery cell arranged in the shell, and a top cover closed on the opening of the shell, and there are two structures for electrically connecting the pole tabs on the battery cell with the pole posts on the top cover. One is that the pole tabs are connected to the pole posts through adapters. In this way, since the pole tabs and the pole posts have a large spatial redundancy in the connection direction, the energy density of the battery will be lower. In another way, the pole tabs are connected to the pole posts through pins. In this way, the welding head needs to be frequently adjusted according to the bending of the pole tabs so that the pole tabs are welded and fixed on the pins, which makes it difficult to ensure the consistency and efficiency of the pole tab welding.
[0072] In order to solve the technical problems mentioned in the background technology, the present invention provides a welding structure of a pole lug, a battery and a pole lug welding process. In the welding structure of the pole lug, a pin is arranged between a battery cell and a bending portion, and the bending portion is welded to the pin, and a pre-welding surface of the bending portion has a width of 4mm-8mm in a first direction and a length of 37mm-41mm perpendicular to the first direction. It can be seen that by limiting the length and width of the pre-welding surface of the bending portion, the area of the pre-welding surface can be limited. Therefore, when the bending portion of the pole lug is welded to the pin, it is only necessary to enable the welding head to weld the bending portion of the pole lug within the area of the pre-welding surface, without the need to frequently adjust the welding head, which can not only improve the efficiency of the pole lug welding, but also improve the consistency of the pole lug welding.
[0073] The present application is described in detail below through specific embodiments:
[0074] See also Figure 1 , Figure 2 and Figure 3 The embodiment of the present application provides a welding structure 100 of a pole ear, wherein the welding structure 100 of the pole ear comprises at least two battery cells 110, at least two pole ears 120 and a pin 130, wherein the at least two pole ears 120 correspond to the at least two battery cells 110 one by one, each pole ear 120 comprises a connecting portion 121 and a bending portion 122 connected by bending, an end of the connecting portion 121 away from the bending portion 122 is connected to the end surface of the corresponding battery cell 110, and the bending portions 122 of two adjacent pole ears 120 of the at least two pole ears 120 are parallel to the first direction. The two pole ears 120 extend toward each other, and there is an insertion gap 123 between the bent portions 122 extending toward each other in two adjacent pole ears 120 and the battery cell 110, and the first direction is the thickness direction of the battery cell 110; the pin 130 is inserted in the insertion gap 123, and the bent portion 122 is welded to the pin 130, and the pre-weld printed surface 124 of the bent portion 122 of each pole ear 120 has a width a1 in the first direction and in a direction parallel to the end face of the battery cell 110, and a length b1 in a direction perpendicular to the first direction, 4mm≤a1≤8mm, and 37mm≤b1≤41mm.
[0075] It should be noted that the first direction mentioned above refers to Figure 1 The direction indicated by the X arrow in the middle is perpendicular to the first direction. Figure 1 The direction indicated by the Y arrow in the figure. The battery cell 110 can be a laminated battery cell or a wound battery cell. For example, when the battery cell is a laminated battery cell, and the tab 120 of the laminated battery cell is a full tab, each layer of the laminate is connected with a tab 120. Since there is a gap between two adjacent tabs 120, in order to facilitate the welding of the tabs 120, the tabs 120 need to be squeezed and bent in the first direction or in the direction opposite to the first direction. The above-mentioned pre-welding surface 124 refers to the area where the ultrasonic pre-welding of the bending portion 122 is performed. Since the length of the pre-welding surface 124 is b1 and the width is a1, the area of the pre-welding surface 124 is b1×a1.
[0076] In the forming process of the battery cell 110, ultrasonic welding is used to form a pre-weld surface 124 after the positive electrode sheet, the negative electrode sheet and the diaphragm are stacked. Each layer of the electrode sheet will have a portion of the exposed electrode ear 120. In order to facilitate the connection of the electrode ears 120 of each layer of the electrode sheet with the pin 130 respectively, so that electrical conduction can be achieved between the electrode ears 120 and the pin 130, it is necessary to use ultrasonic welding to weld and fix the electrode ears 120 of all layers. Preferably, a rectangular welding head is used for ultrasonic welding, so the pre-weld surface formed is rectangular and has a certain length-to-width ratio. It is worth noting that the electrode ears 120 in this embodiment include positive electrode ears and negative electrode ears, which are respectively arranged on the two opposite end faces of the battery cell 110, that is, the at least two electrode ears 120 mentioned above correspond one-to-one to at least two battery cells 110. It should be understood that one electrode ear 120 is arranged on one battery cell 110 (specifically, the positive electrode ear and the negative electrode ear are respectively arranged on the two opposite end faces of the battery cell 110).
[0077] In this embodiment, by welding the bent portion 122 to the pin 130 and the pin 130 being located between the bent portion 122 and the end surface of the battery cell 110 , the distance between the top cover and the battery cell can be reduced, thereby improving the energy density of the battery. In addition, by setting the pre-welding surface 124 of the bending portion 122 to have a width a1 in the first direction and a length b1 perpendicular to the first direction, 4mm≤a1≤8mm, and 37mm≤b1≤41mm, the area of the pre-welding surface 124 of the bending portion 122 can be limited, thereby limiting the pre-welding range of the welding head. Therefore, when welding the bending portion 122 of the pole lug 120 to the pin 130, it is only necessary to enable the welding head to weld the bending portion 122 of the pole lug 120 within the area of the pre-welding surface 124. On the one hand, there is no need to frequently adjust the welding head, thereby improving the efficiency of the welding of the pole lug 120. On the other hand, the consistency of the fusion depth and fusion width of the welding surface of the bending portion 122 of the pole lug 120 can be improved, thereby improving the consistency of the welding of the pole lug 120.
[0078] In addition, when the length b1 of the pre-welding surface 124 is less than 37 mm and the width a1 is less than 4 mm, the area of the pre-welding surface 124 will be too small. When the area of the pre-welding surface 124 is too small, the range of laser welding in the pre-welding surface 124 will also become smaller. If a complete laser welding track cannot be formed, a virtual weld will exist between the tab 120 and the pin 130, thereby affecting the welding effect between the bending portion 122 of the tab 120 and the pin 130. When the length b1 of the pre-welding surface 124 is greater than 41 mm and the width a1 is greater than 8 mm, the welding effect will increase. The length of the tab 120 makes the tab 120 too long, which causes the bent portion 122 to exceed the center of the end face of the battery cell 110, and easily causes a short circuit between the bent portions 122 located on the opposite sides of the end face of the battery cell 110. Therefore, through comprehensive consideration, 4mm≤a1≤8mm, and 37mm≤b1≤41mm are made. In this way, it can avoid that the welding effect between the bent portion 122 of the tab 120 and the pin 130 is affected by the small area of the pre-weld printed surface 124, and the short circuit of the bent portion 122 can be avoided to affect the normal use of the battery 200.
[0079] For example, a1 may be 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, etc., and b1 may be 37 mm, 38 mm, 39 mm, 40 mm, 41 mm, etc.
[0080] In particular, when a1=6mm and b1=39mm, the area of the pre-welding surface 124 is better. In the pre-welding surface 124, when the tab 120 is a full tab 120, the bent portions 122 of the stacked multiple tabs 120 in the full tab 120 can be welded, which can not only ensure the pre-welding effect of the tab 120, but also further improve the consistency and efficiency of welding between the bent portion 122 of the tab 120 and the pin 130. When applied to automatic welding, it is only necessary to control the welding head of the welding device such as ultrasonic welding to weld in the pre-welding surface 124, thereby improving the efficiency and accuracy of pre-welding.
[0081] After the pre-welding of the bent portion 122 of the tab 120 is completed, the pre-welded bent portion 122 of the tab 120 needs to be welded to the pin 130. In some possible embodiments, see Figure 4 The effective soldering surface 125 between the bent portion 122 and the pin 130 has a width a2 in the first direction and a width a3 in the second direction (i.e. Figure 4 The length of the second direction (in the direction indicated by the y arrow) is b2, 1.5mm≤a2≤3mm, and 33mm≤b2≤39mm, and the second direction is parallel to the first direction and the end surface of the battery cell 110.
[0082] The effective soldering surface 125 refers to the area where the bending portion 122 and the lead 130 are actually soldered.
[0083] Specifically, when a2 is less than 1.5 mm and b2 is less than 33 mm, the effective weld surface 125 between the bent portion 122 of the tab 120 and the pin 130 will be smaller, thereby affecting the welding stability between the bent portion 122 of the tab 120 and the pin 130. In addition, when a2 is less than 1.5 mm, due to the small welding width, bubbles and slag residues are likely to appear during the welding process between the bent portion 122 and the pin 130, resulting in excessively high protrusions on the welding surface, which in turn leads to a decrease in the weld width and depth on the welding surface. Insufficient to affect the welding effect between the bent portion 122 and the pin 130. When a2 is greater than 3mm and b2 is greater than 39mm, since the area of the effective welding surface 125 between the bent portion 122 of the tab 120 and the pin 130 is relatively large, there is an area of the pre-welding surface 124 that exceeds the bent portion 122 of the tab 120. In this case, it will affect the welding effect between the bent portion 122 of the tab 120 and the pin 130, and the conductive capacity between the tab 120 and the pin 130, thereby affecting the charging performance of the battery.
[0084] Based on this, through comprehensive consideration, 1.5mm≤a2≤3mm, and 33mm≤b2≤39mm, so that it can avoid affecting the welding stability between the bending portion 122 of the tab 120 and the pin 130 due to the small area of the effective welding surface 125 between the bending portion 122 of the tab 120 and the pin 130, and can improve the penetration depth and width of the welding surface, thereby improving the welding effect between the bending portion 122 and the pin 130, and can also improve the conduction capacity between the tab 120 and the pin 130, thereby improving the charging performance of the battery 200.
[0085] In addition, a2 can be 1.5mm, 2mm, 2.5mm, 3mm, etc., and b2 can be 33mm, 34mm, 35mm, 36mm, 37mm, 38mm, 39mm, etc.
[0086] In particular, when a2=2mm and b2=35mm, the area of the effective weld surface 125 between the bending portion 122 of the tab 120 and the pin 130 is better. At the same time, when a2=2mm, the welding surface can have an effective weld width of more than 1.5mm, thereby further improving the welding effect between the bending portion 122 and the pin 130.
[0087] In some possible embodiments, the pin 130 is a copper pin, and the thickness of the copper pin is m1, 1.8 mm≤m1≤2.3 mm; or, the pin 130 is an aluminum pin, and the thickness of the aluminum pin is m2, 2.8 mm≤m2≤3.3 mm.
[0088] When the thickness of the copper pin is less than 1.8 mm, the structural strength of the copper pin is low, thereby affecting the welding effect between the copper pin and the bent portion. In addition, the thinner copper pin can also affect the current carrying capacity of the copper pin. When the thickness of the copper pin is greater than 2.3 mm, it is not conducive to the high energy density design of the battery. Therefore, the thickness of the copper pin is between 1.8 mm and 2.3 mm.
[0089] In addition, m1 can be 1.8mm, 1.9mm, 2.0mm, 2.1mm, 2.2mm, 2.3mm, etc.
[0090] Similarly, when the thickness of the aluminum pin is less than 2.8mm, the structural strength of the aluminum pin is low, thereby affecting the welding effect between the aluminum pin and the bent portion. In addition, the thinner aluminum pin can also affect the current carrying capacity of the aluminum pin. When the thickness of the aluminum pin is greater than 3.3mm, it is not conducive to the high energy density design of the battery. Therefore, the thickness of the aluminum pin is between 2.8mm and 3.3mm.
[0091] In addition, m2 can be 2.8mm, 2.9mm, 3.0mm, 3.1mm, 3.2mm, 3.3mm, etc.
[0092] It is worth noting that since the tabs include a positive tab and a negative tab, and the positive tab and the negative tab are made of different materials, therefore, considering the conduction between the tab 120 and the pin 130, the positive pin and the negative pin can be made of different materials. For example, the positive pin is an aluminum pin and the negative pin is a copper pin.
[0093] In some possible embodiments, no active material layer is disposed on the bending portion 122 .
[0094] It should be noted that no active material layer is provided on the above-mentioned bending portion 122. It should be understood that the active material layer on the bending portion 122 on the positive electrode tab is formed by positive electrode materials, such as lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel oxide, nickel cobalt manganese oxide, etc., and the active material layer on the bending portion 122 on the negative electrode tab is formed by negative electrode materials, such as graphite, lithium titanate, or graphite, etc.
[0095] Since no active material layer is provided on the bending portion 122 , on the one hand, during the charging and discharging process of the battery, the bending portion 122 does not participate in the charging and discharging reaction in the electrolyte; on the other hand, providing an active material layer on the bending portion 122 will affect the welding effect between the bending portion 122 and the pin 130 .
[0096] See also Figure 5The embodiment of the present application also provides a battery 200, which includes a shell 220, a battery cell 110, a welding structure 100 of the pole ear and a top cover 230, wherein the shell 220 is hollow inside and has an opening 221 connected to the inside of the shell 220; the battery cell 110 is arranged inside the shell 220, and the end face of the battery cell 110 is opposite to the side wall of the shell 220, and the side wall of the battery cell 110 is opposite to the opening 221; the pin 130 extends toward the inside of the shell 220 to be inserted in the insertion gap 123; the top cover 230 is installed in the opening 221, and the top cover 230 includes a pole 231, and the pole 231 is connected to the pin 130.
[0097] Among them, the welding structure 100 of the pole ear in the embodiment of the present application can be the same as the structure of any of the welding structures 100 of the pole ears in the above embodiments, and can bring the same or similar beneficial effects. For details, please refer to the description in the above embodiments, and the embodiments of the present application will not be repeated here.
[0098] Since the end face of the battery cell 110 is opposite to the side wall of the housing 220, the side wall of the battery cell 110 is opposite to the opening 221, the pin 130 extends toward the inside of the housing 220 to be inserted in the insertion gap 123, and the pole 231 is connected to the pin 130, therefore, in the direction of the opening 221, the top cover 230 is opposite to the side wall of the battery cell 110, and no space is reserved in this direction for the connection between the tab 120 and the adapter and the adapter and the pole 231. It can be seen that space is saved in the direction of the opening 221, thereby improving the energy density of the battery 200. In addition, the tab 120 can be electrically connected to the pole 231 through the pin 130.
[0099] In addition, since the battery 200 in this embodiment includes the electrode tab welding structure 100 in the above embodiment, the comprehensive performance of the battery 200 is improved.
[0100] See also Figure 6 The embodiment of the present application further provides a welding process for a pole tab 120, which is used to weld the above-mentioned welding structure 100 of the pole tab. The welding process for the pole tab 120 includes:
[0101] S10, insert the pin into the insertion gap.
[0102] Specifically, the battery cell 110 and the pole ear 120 are fixed (in one case, the pole ear 120 is welded to the end face of the battery cell 110, and in another case, the pole piece of the battery cell 110 is integrally formed with the pole ear 120), and then, the pole ear 120 is bent along a first direction so that the pole ear 120 forms a bending portion 122 and a connecting portion 121 connected between the bending portion 122 and the end face of the battery cell 110, and an insertion gap 123 is provided between the bending portion 122 and the end face of the battery cell 110, and the bending portion 122 can be parallel or approximately parallel to the end face of the battery cell 110, and finally, a portion of the pin 130 is inserted into the insertion gap 123 to complete the pre-installation of the pin 130.
[0103] It should be noted that the thickness of the pin 130 is not limited. For example, when the pin 130 is a copper pin, the thickness of the copper pin is 2 mm. When the pin 130 is an aluminum pin, the thickness of the aluminum pin is 3 mm.
[0104] S20, using a moving and swinging welding track to weld the bent portion to the pin.
[0105] Specifically, the bending portion 122 is welded to the pin 130 using a laser welding device 300, see Figure 7 The laser welding device 300 includes a collimator 310, a focusing lens 320 and a galvanometer 330 arranged in sequence along the optical path, wherein the collimator 310 is used to collimate the laser beam, the focusing lens 320 is used to focus the laser beam emitted from the collimator 310, and the galvanometer 330 can control the trajectory of the emitted laser beam, that is, the trajectory of the laser beam forms a welding trajectory in the direction of movement and vibration. Among them, the above-mentioned movement and swing should be understood, taking the laser beam moving along the first direction as an example, movement refers to the movement of the laser beam along the first direction, and swing refers to the movement of the laser beam in a direction perpendicular to the first direction and parallel to the end face of the battery cell.
[0106] Therefore, by adding vibration to the moving welding trajectory, the bending portion 122 and the pin 130 can be welded at a faster speed, and the metallographic effect of the welding point can be optimized, so as to achieve the purpose of improving the quality of laser welding by optimizing the welding trajectory.
[0107] Of course, during the welding process of the tab 120 and the pin 130, see Figure 7 The laser welding device 300 can perform vertical welding on the tab 120 and the pin 130 (i.e., the welding surfaces of the tab 120 and the pin 130 are horizontal, and the laser beam emitted by the laser welding device 300 is emitted in a vertical direction toward the welding surfaces of the tab 120 and the pin 130), see Figure 8Alternatively, the tab 120 and the pin 130 may be horizontally welded (i.e., the welding surfaces of the tab 120 and the pin 130 are vertical, and the laser beam emitted by the laser welding device 300 is emitted toward the welding surfaces of the tab 120 and the pin 130 in a horizontal direction).
[0108] Specifically, when the battery cell 110 is small in size, it is convenient to carry and rotate it during welding, and it will not damage the battery cell 110. Therefore, vertical welding is usually used to weld the tab 120 and the pin 130. When the battery 200 is large in size, since the battery cell 110 needs to be carried and rotated during welding, which may easily damage the battery cell 110, horizontal welding is used to weld the tab 120 and the pin 130.
[0109] In addition, the spot of the laser beam emitted by the laser welding device 300 can be a circular spot or an annular spot. For example, when the annular light plate is welded to an aluminum pole ear, the inner ring power of the laser beam of the annular spot emitted by the laser welding device 300 is 1500w, and the outer ring power is 2000w. When the annular light plate is welded to a copper pole ear, the inner ring power of the laser beam of the annular spot emitted by the laser welding device 300 is 1800w, and the outer ring power is 2000w. The welding speed of the laser welding device 300 is 400mm / s. In this way, the corresponding standards of melt width and melt depth can be met, and the obtained welding metallographic structure is complete and free of bubbles and slag.
[0110] In addition, there are various welding trajectories formed by movement and swinging. In some possible embodiments, see Fig. 9 , Fig.10 and Fig.11 The welding trajectory is one of a sine curve, a double helix curve, and a cross straight line.
[0111] Since the welding trajectory of the sine curve is a smooth arc transition at the bend, it can reduce welding spatter and optimize the appearance of the weld line. In addition, since there are more welding overlaps in the welding trajectory of the double helix curve, the welding depth can be increased, which can be applied to the welding of thicker materials. In addition, since the welding trajectory of the cross straight line has a better distribution uniformity, it can optimize the welding pool and reduce the porosity slag inside the welding pool.
[0112] For example, a welding trajectory using a sine curve can be used to weld copper pole tabs within 100 layers; a welding trajectory using a double helix curve can be used to weld copper pole tabs within 180 layers.
[0113] In some possible embodiments, see Fig.12 and Fig.13The welding trajectory is any two of a sine curve, a double helix curve, and a cross straight line, or the welding trajectory includes a sine curve, a double helix curve, and a cross straight line.
[0114] Since the sinusoidal welding trajectory can reduce welding spatter and optimize the appearance of the weld line, the double helix curve welding trajectory can increase the welding depth and is used for welding thicker materials, the cross straight line welding trajectory can optimize the welding molten pool and reduce the porosity slag inside the welding molten pool, and the cross straight line welding trajectory can be used for primer, therefore, when any two welding trajectories of the sinusoidal curve, double helix curve, and cross straight line are combined, the effects of each welding trajectory can be superimposed, and the welding metallographic structure can be further optimized to avoid overheating of welding, thereby reducing the risk of thermal runaway during welding.
[0115] When the welding trajectory is a combination of a sine curve, a double helix curve and a cross straight line, it can add the effects of each welding trajectory while reducing welding protrusions, welding surface pores, metallographic bubbles and slag, thereby improving the fullness of the weld line and the welding metallography, making the welding metallography as free of bubbles and slag as possible.
[0116] In some possible embodiments, before welding the bent portion 122 to the pin 130 using a moving and swinging welding track, the welding process includes:
[0117] The pins 130 and the tabs 120 are clamped and positioned.
[0118] The bending portion 122 is pre-welded by ultrasonic welding.
[0119] Specifically, the bending portion 122 is pre-welded by an ultrasonic welding device 400, wherein Fig.14 The ultrasonic welding device 400 includes a transducer 410, an amplitude modulator 420 and a welding head 430. The transducer 410 can convert high-frequency electrical energy into mechanical vibration. That is to say, by setting the transducer 410, the welding head 430 can be vibrated. The amplitude modulator 420 can control the amplitude of the welding head 430 during the vibration process, thereby achieving the purpose of optimizing the welding trajectory of the welding head 430.
[0120] Thus, the welding head 430 can vibrate at a specific frequency and specific amplitude to pre-weld the bent portion 122 of the tab 120 , thereby welding the multi-layered bent portion 122 into a whole, in preparation for the laser welding device 300 to weld the bent portion 122 to the pin 130 .
[0121] In some possible embodiments, welding the bent portion 122 to the pin 130 using a moving and swinging welding track includes: welding the bent portion 122 to the pin 130 using laser welding, and the width of the laser welding is greater than or equal to 2 mm.
[0122] When the width of the laser weld is less than 2 mm, it is difficult to ensure the effective molten width of the welding surface of the bend 122. In other words, when the width of the laser weld is less than 2 mm, due to the narrow effective molten width of the welding surface of the bend 122, bubbles and slag residues are easily generated on the welding surface of the bend 122 during the laser welding process, which makes the welding surface convex, thereby affecting the welding quality of the laser weld. Based on this, limiting the width of the laser weld to 2 mm or more can ensure that the effective molten width of the welding surface of the bend 122 is 1.5 mm or more, so that bubbles and slag residues on the welding surface can be reduced, thereby improving the welding quality of the laser weld.
[0123] In some possible embodiments, the tab welding process further includes:
[0124] Before welding, the welding surface between the bent portion 122 and the pin 130 is a smooth surface. Since the smooth surface can cause the reflection of the laser beam, the risk of adverse effects such as welding penetration caused by laser welding on the welding surface can be reduced, thereby improving the welding effect between the bent portion 122 and the pin 130.
[0125] It should be noted that the welding surface after the bending portion 122 and the pin 130 are welded and fixed is not limited.
[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A welding structure of a tab, characterized in that: include: At least two cells; At least two pole lugs, at least two of the pole lugs correspond to at least two of the battery cells one by one, each of the pole lugs comprises a connecting portion and a bending portion connected by bending, one end of the connecting portion away from the bending portion is connected to the end face of the corresponding battery cell, the bending portions of two adjacent pole lugs of at least two of the pole lugs extend toward each other in a direction parallel to a first direction, and an insertion gap is provided between the bending portions extending toward each other in two adjacent pole lugs and the end face of the battery cell, and the first direction is a thickness direction of the battery cell; The pin is inserted in the insertion gap, and the bent portion is welded to the pin, the pre-welded surface of the bent portion of each of the tabs has a width a1 in the first direction and a length b1 in a direction perpendicular to the first direction and parallel to the end face of the battery cell, 4mm≤a1≤8mm, and 37mm≤b1≤41mm.
2. The welding structure of the electrode tab according to claim 1, characterized in that: The effective welding surface between the bending portion and the pin has a width a2 in the first direction and a length b2 in the second direction, 1.5mm≤a2≤3mm, and 33mm≤b2≤39mm, and the second direction is parallel to the first direction and the end face of the battery cell.
3. The welding structure of the electrode tab according to claim 1, characterized in that: The pin is a copper pin, and the thickness of the copper pin is m1, 1.8mm≤m1≤2.3mm; or, The pin is an aluminum pin, and the thickness of the aluminum pin is m2, 2.8mm≤m2≤3.3mm.
4. A battery, characterized in that: include: a housing, the interior of the housing being hollow and having an opening communicating with the interior of the housing; The welding structure of the pole lug according to any one of claims 1 to 3, wherein the battery cell in the welding structure of the pole lug is arranged inside the shell, and the end face of the battery cell is opposite to the side wall of the shell, and the side wall of the battery cell is opposite to the opening; A top cover is installed on the opening, and the top cover includes a pole, and the pole is connected to a pin in the welding structure of the pole ear.
5. A tab welding process, characterized in that: The tab welding process is used to weld the tab welding structure according to any one of claims 1 to 3, and the process comprises: Inserting the pin into the insertion gap; The bent portion is welded to the pin using a moving and swinging welding track.
6. The tab welding process according to claim 5, characterized in that: The welding trajectory is one of a sine curve, a double helical curve, and a cross straight line.
7. The tab welding process according to claim 5, characterized in that: The welding trajectory is any two of a sine curve, a double helical curve, and a cross straight line, or the welding trajectory includes a sine curve, a double helical curve, and a cross straight line.
8. The tab welding process according to claim 5, characterized in that: Before the bending portion is welded to the pin by using a moving and oscillating welding track, the process includes: Clamping and positioning the pin and the tab; The bending portion is pre-welded by ultrasonic welding.
9. The tab welding process according to claim 5, characterized in that: The method of welding the bent portion to the pin by using a moving and swinging welding track includes: The bent portion is welded to the pin by laser welding, and the width of the laser welding is greater than or equal to 2 mm.
10. The tab welding process according to claim 5, characterized in that: The process also includes: Before welding, the welding surfaces of the bent portion and the pin are both smooth surfaces.
Citation Information
Patent Citations
Secondary battery
CN105762322A
Soft package battery cell module tab welding method and welding tool
CN114069166A
Power lithium cell electricity core and header connection structure
CN205335338U
Secondary electricity core
CN206134803U
Battery and electronic device
CN218975498U
Cited By
Battery monomer and electric equipment
CN119650978A
Energy storage apparatus and electrical device
WO2026113715A1