Hollow shell-shell structure geopolymer microsphere and preparation method and application thereof
The preparation of hollow shell-shell structure polymer microspheres through dispersion-suspended-curing method has solved the problems of complexity and insufficient performance of the hollow microsphere preparation method in the prior art, and achieved efficient and simple preparation of hollow microspheres with high efficiency and high quality Mechanical strength and excellent adsorption and catalytic properties.
Patent Information
- Application Number
- CN202310271371.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-20
AI Technical Summary
The existing hollow microsphere preparation methods are complicated to operate, lack mechanical strength, difficult to control the structural size, uneven pore size distribution, and high cost.
The hollow shell-shell structure polymer microspheres are prepared by dispersion-suspended-curing method. By stirring the gel material with alkali or acid activation activity with water and the exciter into a uniform adhesive slurry, water is added without mutual dissolution. The solvent is cured in hot silicone oil and then calcined to form hollow microspheres with thin shell structure, uniform pore size distribution and high specific surface area.
The preparation of hollow microspheres with good spherical shape has been achieved, with a thickness of 25-75μm and a pore inner diameter of 15-45μm. The pore volume is high and the specific surface area is large. It has the characteristics of high mechanical strength, high temperature resistance, corrosion resistance and radiation resistance. , suitable for adsorption and catalysis fields.
Smart Images

Figure CN116474755B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of geopolymer microspheres, and in particular to a hollow shell-shell structured geopolymer microsphere and a preparation method and application thereof. Background Art
[0002] Since 2002, the synthesis of hollow microspheres has attracted more and more attention in the field of materials science. Hollow microspheres have the advantages of low density, good dispersibility, large specific surface area, regular structure, and adjustable size. They are widely used in encapsulation, catalysis, energy storage, adsorption, magnetism, optics, and biomedicine.
[0003] Methods for preparing hollow microspheres include: high temperature dissolution method, spray drying method, template method, self-assembly method and hydrothermal method. In the prior art, Ni / Si composite hollow microspheres were prepared by template method, which had high catalytic activity and excellent selectivity for the reduction of acetone to 2-propanol, with a conversion rate of 70% and a selectivity of 82.7%. In the prior art, copper oxide hollow microspheres were also prepared by low temperature liquid phase method, and the maximum adsorption capacity of As(III) was 81.45 mg / g. Traditionally, the preparation of hollow microspheres is mainly based on template method. Hard templates are mainly synthesized by using organic template agents to synthesize hollow microspheres, and finally the core of the template agent is dissolved by high temperature calcination or chemical method to generate cavities. Some scholars also synthesized hollow spheres by using hard inorganic spheres such as silica as templates, and the thickness of the shell of the hollow spheres is relatively uniform, and the inner diameter of the sphere can be controlled by the size of the template particles. Soft templates such as emulsion droplets, surfactant micelles, bubbles, polymer vesicles, etc. can also be used to synthesize hollow spheres. In addition, hollow titanium dioxide microspheres are also synthesized by a template-free method in the prior art.
[0004] However, the above preparation methods have the disadvantages of complicated operation, lack of mechanical strength, difficult to control structural size, and uneven pore size distribution. Therefore, it is necessary to develop a method that is simple and efficient to operate and has good product performance.
[0005] Compared with the above materials, geopolymer materials have the advantages of high mechanical strength, simple preparation process, low cost, and green environmental protection. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a hollow shell-shell structured geopolymer microsphere and a preparation method and application thereof. The hollow shell-shell structured geopolymer microsphere prepared by the present invention using geopolymer technology is an inorganic substance with stable performance, large porosity, high specific surface area, uniform pore size distribution, high temperature resistance, corrosion resistance, acid and alkali resistance and radiation resistance. It can be used as an excellent carrier to load some inorganic and organic substances with excellent performance on its surface, and can obtain excellent adsorption and catalytic performance, thereby solving the problems mentioned in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solution: a hollow shell-shell structured geopolymer microsphere, wherein the hollow shell-shell structured geopolymer microsphere is prepared by a dispersion-suspension-solidification method, the hollow shell-shell structured geopolymer microsphere has good sphericity and a thin shell structure, the shell wall thickness is 25 to 75 μm, and the microsphere pore volume can reach 0.78 cm 3 / g, the specific surface area can reach 99.468m 2 / g, the pore inner diameter is 15-45μm, and the particle size is 30-300μm.
[0008] In addition, to achieve the above object, the present invention also provides the following technical solution: a method for preparing hollow shell-shell structured geopolymer microspheres, comprising the following steps:
[0009] S1. A gel material having alkali excitation activity or acid excitation activity, water and an exciter are stirred and dispersed in a certain proportion to form a uniform adhesive slurry A;
[0010] S2, adding a certain amount of water-immiscible solvent to slurry A, and dispersing it into uniform slurry B in a stirrer at a certain speed;
[0011] S3, pour slurry B into hot silicone oil (or a water-immiscible solvent) dispersed at high speed by a stirrer, disperse it into balls, and put it into an oven for curing and solidification;
[0012] S4, filtering, washing and drying the cured balls to obtain hollow microsphere precursors;
[0013] S5. The hollow microsphere precursor is calcined and sieved to obtain hollow shell-shell structured geopolymer microspheres.
[0014] Preferably, in step S1, the mass ratio of the gel material having alkali excitation activity or acid excitation activity, the exciter, and water is 4-20:6-20:2-10.
[0015] Preferably, in step S2, the mass ratio of the adhesive slurry A to the water-immiscible solvent is 1:0.005-0.3.
[0016] Preferably, the gel material with alkali activation or acid activation is one or more of blast furnace slag, granulated phosphorus slag, steel slag, volcanic ash, manganese slag, metakaolin, red mud, fly ash, rice husk ash, and condensed silica ash; the activator includes an alkaline activator and an acid activator; the alkaline activator is sodium / potassium water glass dry powder, sodium / potassium water glass liquid, sodium / potassium hydroxide, non-silicate weak acid salt (M 2 CO 3 、M 2 SO 3 、M 3PO 4 , MF, etc.), aluminate (M 2 O·nSiO 2 ), aluminosilicate (M 2 O.Al 2 O 3 ·[2-6]SiO 2 ) or strong acid salts other than aluminosilicates (M 2 SO 4 ); the acidic activator is one or more of phosphoric acid, nitric acid, hydrochloric acid, acetic acid, and sulfuric acid.
[0017] Preferably, the water-immiscible solvent is one or more of liquid paraffin, silicone oil, polyethylene glycol, peanut oil, and waste cooking oil.
[0018] Preferably, in step S2, the speed of the stirrer is 300-4000 rpm / min, and the stirring time is 0.5-10 min; in step S3, the speed of the stirrer is 300-2800 rpm / min, and the temperature of the hot silicone oil is 40-280°C.
[0019] Preferably, the curing and curing temperature in step S3 is 40 to 280° C., and the curing time is 0.5 to 48 hours.
[0020] Preferably, the calcination temperature in step S5 is 200-1700° C., and the calcination time is 0.5-24 h.
[0021] In addition, to achieve the above purpose, the present invention also provides the following technical solution: an application of a hollow shell-shell structured geopolymer microsphere, wherein the hollow shell-shell structured geopolymer microsphere is used as an adsorption material or a catalytic material in the field of adsorption and catalysis.
[0022] The beneficial effects of the present invention are as follows: the present invention adds a water-immiscible solvent to the geopolymer slurry that has been stirred and dispersed uniformly, and continues to stir uniformly, and then pours the uniformly dispersed slurry into high-speed dispersed hot silicone oil (a water-immiscible solvent), and obtains the desired hollow microspheres after curing, solidification, cleaning, filtering, drying, and calcining. Compared with the materials in the prior art, geopolymer materials have the advantages of high mechanical strength, simple preparation process, low cost, and green environmental protection. Compared with the traditional method for preparing hollow microspheres, the present invention has simple synthesis steps, easy to control the operation process, and the prepared hollow microspheres have good sphericity, thin shell walls (25-75μm), large pore inner diameters (15-45μm), and total pore volumes (0.78cm 3 / g) and high specific surface area (99.468m 2 / g), high efficiency, controllable particle size (30-300μm), and excellent properties such as high strength, high temperature resistance, corrosion resistance, and stable chemical properties. It can be used as an excellent adsorption material and catalytic material. This method has great advantages and application prospects in the preparation of hollow microspheres and in the fields of adsorption and catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 1-2;
[0024] Figure 2 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 3-4;
[0025] Figure 3 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 5-6;
[0026] Figure 4 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 7;
[0027] Figure 5 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 8;
[0028] Figure 6 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 9;
[0029] Figure 7 This is an optical microscope picture of the hollow shell-shell structured geopolymer microspheres obtained in Example 10. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] Stir 42g of metakaolin, 10g of water glass and 1g of water into a uniform slurry using a glass rod;
[0033] 0.36 g of liquid paraffin was added to the uniform slurry, and then stirred in a stirrer at 300 rpm / min for 1 min;
[0034] Pour the stirred slurry into 65℃ silicone oil rotating at 300rpm / min, and place it in a 65℃ oven for curing for 6h;
[0035] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0036] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 200° C. for 1 hour and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0037] The hollow shell-shell structured geopolymer microspheres obtained in Example 1 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 1 A, A1, by Figure 1 A and A1 show that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 30 μm and an average pore size of 32 μm.
[0038] Example 2
[0039] Stir 10g of metakaolin, 3g of water glass and 5g of water into a uniform slurry using a glass rod;
[0040] 5.4 g of liquid paraffin was added to the uniform slurry, and then stirred in a stirrer at 1000 rpm / min for 10 min;
[0041] Pour the stirred slurry into 85℃ silicone oil rotating at 2800rpm / min, and place it in an 85℃ oven for curing for 2h;
[0042] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0043] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 900° C. for 10 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0044] The hollow shell-shell structured geopolymer microspheres obtained in Example 2 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 1 B, B1, by Figure 1 B and B1 show that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 32 μm and an average pore diameter of 40 μm.
[0045] Weigh 0.06 g of the hollow shell-shell geopolymer microspheres obtained and add them to 100 mL of 300 ppm Pb 2+ The solution was shaken in a shaker for 2 h, and the maximum adsorption capacity was 529.67 mg / g. The hollow shell-shell structure geopolymer microspheres prepared in this example had a higher adsorption capacity for Pb than other hollow microspheres. 2+ The removal rate and adsorption effect are better, and the recycling performance is good.
[0046] Example 3
[0047] Stir 15 g of metakaolin, 14 g of sodium hydroxide and 4 g of water into a uniform slurry using a glass rod;
[0048] 0.32 g of silicone oil was added to the uniform slurry, and then stirred in a stirrer at 500 rpm / min for 8 min;
[0049] Pour the stirred slurry into 85℃ silicone oil rotating at 600rpm / min, and put it into an 85℃ oven for curing for 1h;
[0050] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0051] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 600° C. for 3 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0052] The hollow shell-shell structured geopolymer microspheres obtained in Example 3 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 2 A(A1), given by Figure 2 A(A1) shows that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 25 μm and an average pore size of 45 μm.
[0053] Example 4
[0054] Stir 9 g of metakaolin, 16 g of sodium hydroxide and 6 g of water into a uniform slurry using a glass rod;
[0055] 6.20 g of silicone oil was added to the uniform slurry, and then stirred in a stirrer at 2000 rpm / min for 2 min;
[0056] Pour the stirred slurry into 85℃ silicone oil rotating at 1500rpm / min, and place it in an 85℃ oven for curing for 1h;
[0057] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0058] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 600° C. for 3 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0059] The hollow shell-shell structured geopolymer microspheres obtained in Example 4 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 2 B(B1), by Figure 2B(B1) shows that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 28 μm and an average pore diameter of 40 μm.
[0060] Weigh 0.1 g of the hollow shell-shell geopolymer microspheres and add them to 100 mL of 50 mg / L Sr 2+ The solution was shaken in a shaker for 2 h, and the maximum adsorption capacity was 106.28 mg / g. The hollow shell-shell geopolymer microspheres prepared in this example have a higher adsorption capacity for Sr2 than other hollow microspheres. + The removal rate and adsorption effect are better, and the recycling performance is good.
[0061] Example 5
[0062] Stir 11g of metakaolin, 14g of water glass and 5g of water into a uniform slurry using a glass rod;
[0063] 0.29 g of polyethylene glycol (200) was added to the homogeneous slurry, and then stirred in a stirrer at 600 rpm / min for 7 min;
[0064] Pour the stirred slurry into 85℃ silicone oil rotating at 800rpm / min, and put it into an 85℃ oven for curing for 8h;
[0065] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0066] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 400° C. for 4 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0067] The hollow shell-shell structured geopolymer microspheres obtained in Example 5 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 3 A(A1), given by Figure 3 A(A1) shows that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 40 μm and an average pore diameter of 33 μm.
[0068] Example 6
[0069] Stir 20g of metakaolin, 4g of water glass and 4g of water into a uniform slurry using a glass rod;
[0070] 3.6 g of polyethylene glycol (600) was added to the uniform slurry, and then stirred in a stirrer at 1800 rpm / min for 0.5 min;
[0071] Pour the stirred slurry into 85℃ silicone oil rotating at 2500rpm / min, and put it into an 85℃ oven for curing for 8h;
[0072] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0073] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 1000° C. for 0.5 h and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0074] The hollow shell-shell structured geopolymer microspheres obtained in Example 6 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 3 B(B1), by Figure 3 B(B1) shows that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 47 μm and an average pore diameter of 22 μm.
[0075] Example 7
[0076] Stir 3g of metakaolin, 14g of water glass and 6g of water into a uniform slurry using a glass rod;
[0077] 5.75 g peanut oil was added to the homogeneous slurry, and then stirred in a stirrer at 700 rpm / min for 3 min;
[0078] Pour the stirred slurry into 85℃ silicone oil rotating at 600rpm / min, and put it into an 85℃ oven for curing for 8h;
[0079] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0080] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 500° C. for 4 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0081] The hollow shell-shell structured geopolymer microspheres obtained in Example 7 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 4 ,Depend on Figure 4 It can be seen that the hollow shell-shell structured geopolymer microspheres prepared in this embodiment have good sphericity and a thin shell structure, with an average wall thickness of 56 μm and an average pore size of 38 μm. The hollow microspheres have a good degradation effect on tetracycline hydrochloride under ultraviolet light conditions. When the tetracycline hydrochloride concentration is 10 ppm, the solid-liquid ratio is 0.3 g / L, and the hydrogen peroxide concentration is 6 mM, the aluminum degradation reaches 90% in 120 minutes.
[0082] Example 8
[0083] Stir 30 g of metakaolin, 10 g of phosphoric acid and 12 g of water into a uniform slurry using a glass rod;
[0084] 0.42 g of silicone oil was added to the uniform slurry, and then stirred in a stirrer at 1500 rpm / min for 3 min;
[0085] Pour the stirred slurry into 105℃ silicone oil rotating at 2600rpm / min, and place it in a 105℃ oven for curing for 2h;
[0086] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0087] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 1200° C. for 3 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0088] The hollow shell-shell structured geopolymer microspheres obtained in Example 8 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 5 ,Depend on Figure 5 It can be seen that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 50 μm and an average pore size of 29 μm. - It has obvious removal effect, with a removal rate of up to 90% and a maximum adsorption capacity of 190 mg / g.
[0089] Example 9
[0090] 24 g red mud, 6 g slag, 14 g water glass and 8 g water were stirred into a uniform slurry using a glass rod;
[0091] 2.08 g of liquid paraffin was added to the uniform slurry, and then stirred in a stirrer at 2000 rpm / min for 1 min;
[0092] Pour the stirred slurry into 85℃ silicone oil rotating at 1000rpm / min, and place it in an 85℃ oven for curing for 2h;
[0093] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0094] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 500° C. for 3 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0095] The hollow shell-shell structured geopolymer microspheres obtained in Example 9 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 6 ,Depend on Figure 6 It can be seen that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 60 μm and an average pore diameter of 30 μm.
[0096] Weigh 0.03 g of the hollow shell-shell geopolymer microspheres obtained and add them to 30 mL of 50 ppm F - The solution was shaken in a shaker for 2 h, and the maximum adsorption capacity was 76.57 mg / g. The hollow shell-shell structured geopolymer microspheres prepared in this example had a higher adsorption capacity than other hollow microspheres for F - The removal rate and adsorption effect are better, and the adsorption speed is faster.
[0097] Example 10
[0098] Stir 20g of slag, 14g of water glass and 8g of water into a uniform slurry using a glass rod;
[0099] 12.6 g of liquid paraffin was added to the uniform slurry, and then stirred in a stirrer at 1100 rpm / min for 7 min;
[0100] Pour the stirred slurry into 85℃ silicone oil rotating at 400rpm / min, and put it into an 85℃ oven for curing for 2h;
[0101] The cured slurry is filtered, washed and dried to obtain primary hollow shell-shell structured geopolymer microspheres;
[0102] The primary hollow shell-shell structured geopolymer microspheres are then calcined at 600° C. for 10 hours and sieved to obtain the hollow shell-shell structured geopolymer microspheres with different particle sizes.
[0103] The hollow shell-shell structured geopolymer microspheres obtained in Example 10 were observed under an optical microscope, and the obtained OM image is shown in FIG. Figure 7 ,Depend on Figure 7 It can be seen that the hollow shell-shell structured geopolymer microspheres prepared in this example have good sphericity and a thin shell structure, with an average wall thickness of 65 μm and an average pore diameter of 20 μm.
[0104] Comparative Example 1
[0105] Seed emulsion synthesis
[0106] A stirrer, reflux condenser, thermometer and N 2 A certain amount of water, polyvinyl pyrrolidone, methyl methacrylate and methacrylic acid were added to the four-necked flask with an air guide tube, stirred evenly, vacuumed and nitrogen-filled at room temperature for 3 times each, heated to 70°C, and injected with a measured KPS aqueous solution. The reaction was carried out for 6 hours to obtain a milky white poly(methyl methacrylate-methacrylic acid), i.e., P(MMA-MMA) emulsion.
[0107] Seeded emulsion polymerization
[0108] The emulsion obtained above was added to a four-necked flask, styrene and additives were added, the system was stirred and swollen at 30°C for 24h, then the temperature was raised to 80°C, KPS was added in batches to initiate polymerization for 5h, and P(MMA-MMA) / PSt composite emulsion was obtained. The emulsion was cooled, the pH value was adjusted to 12 with 10% KOH by mass, the temperature was raised to 95°C for a certain period of time, and then cooled to room temperature to obtain hollow plastic pigment particles. The pore volume of the obtained hollow microspheres was 0.17cm 3 / g.
[0109] Comparative Example 2
[0110] Dissolve glucose in deionized water, stir thoroughly and transfer to a reactor for hydrothermal reaction at 200℃ for 10h. Cool naturally to room temperature, filter, wash twice with deionized water and anhydrous ethanol respectively, and dry the product at 50℃ for later use.
[0111] Take a certain amount of prepared carbon spheres, add 0.5 mol sodium hydroxide and 500 mL deionized water, and after ultrasonic dispersion and strong stirring, treat with alkali in a 90°C water bath for 2, 4, and 6 hours respectively, filter, wash, and dry for later use.
[0112] The carbon spheres without surface modification and those modified with strong base for 2, 4, and 6 hours were divided into 4 groups and dispersed in 500 mL of deionized water. 4+ Y 3+ It is easier to adsorb on the surface of carbon spheres, so a two-step method is used for impregnation: first, impregnation of Y 3+ solution, and then impregnated with Zr 4+ The solution is immersed in Zr 4+ When the solution is prepared, part of Y pre-adsorbed on the surface of the carbon sphere 3+ Therefore, 0.15 mol of Y(NO 3 ) 3 6H 2 O, and then add 0.15 mol of Zr(NO 3 ) 4 ·5H 2 O, and impregnated for 2 hours under stirring. After impregnation, the product was filtered, washed twice with deionized water and anhydrous ethanol, and dried at 50°C to obtain a dark brown precursor. A two-step calcination method was used. The precursor was first kept at 1200°C for 2 hours in an argon protective atmosphere to form a hard shell; then kept at 750°C for 4 hours to remove the carbon in the core, and then cooled to room temperature to obtain white ZrO 2 Hollow spheres. The specific surface area of the obtained hollow microspheres is 47.90m 2 / g.
[0113] Comparison and verification results
[0114] The hollow microspheres prepared in Examples 1-10 and Comparative Examples 1-2 are compared. It can be seen that the preparation process of the present invention is simple and easy to operate. It only needs to prepare the material into a uniform slurry and pour it into a water-immiscible solvent for solidification. The preparation conditions are not harsh, and no fixed film-forming agent, initiator and pH are required. The preparation process is not greatly affected by external factors (stirring speed, temperature, etc.). And the specific surface area of the hollow microspheres prepared by the present invention (99.46m 2 / g) and pore volume (0.78 cm 3 / g) are relatively large. The present invention utilizes a dispersion-suspension-solidification method to suspend a uniformly dispersed slurry in a dispersion medium in the form of small droplets, so that the periphery is surrounded by the dispersion medium. Due to the fast solidification property of the geopolymer, the wrapped small droplet slurry can form microspheres of different particle sizes by fast solidification under the dispersion of the stirrer, and then a solution immiscible with water is wrapped in the center of the small droplet. After calcining it at a high temperature, the solid microsphere becomes a hollow microsphere with a shell-shell structure, and the particle size distribution, specific surface area and pore volume of the spheres can be controlled by controlling the dispersion speed of the stirrer and the amount of the added solvent immiscible with water.
[0115] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing hollow shell-shell structured geopolymer microspheres, characterized in that: The steps include: S1. A gel material having alkali activation activity or acid activation activity, water and an activator are stirred and dispersed in a certain proportion to form a uniform adhesive slurry A; S2, adding a certain amount of water-immiscible solvent to slurry A, and dispersing it into uniform slurry B in a stirrer at a certain speed; S3, pour slurry B into hot silicone oil dispersed at high speed by a stirrer to disperse it into balls, and put it into an oven for curing and solidification; S4, filtering, washing and drying the cured balls to obtain hollow microsphere precursors; S5. The hollow microsphere precursor is calcined and sieved to obtain hollow shell-shell structured geopolymer microspheres.
2. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the gel material having alkali excitation activity or acid excitation activity, the exciter, and water is 4-20:6-20:2-10.
3. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the adhesive slurry A to the solvent immiscible with water is 1:0.005-0.
3.
4. The preparation method according to claim 1, characterized in that: The gel material with alkali activation activity or acid activation activity is one or more of blast furnace slag, granulated phosphorus slag, steel slag, volcanic ash, manganese slag, metakaolin, red mud, fly ash, rice husk ash, and condensed silica ash; the activator includes an alkaline activator and an acidic activator; the alkaline activator is sodium / potassium water glass dry powder, sodium / potassium water glass liquid, sodium / potassium hydroxide, weak acid salt of non-silicate, aluminate, aluminosilicate or strong acid salt of non-aluminosilicate; the acidic activator is one or more of phosphoric acid, nitric acid, hydrochloric acid, acetic acid, and sulfuric acid.
5. The preparation method according to claim 1, characterized in that: The water-immiscible solvent is one or more of liquid paraffin, silicone oil, polyethylene glycol, peanut oil, and waste cooking oil.
6. The preparation method according to claim 1, characterized in that: In step S2, the rotation speed of the stirrer is 300-4000 rpm / min, and the stirring time is 0.5-10 min; in step S3, the rotation speed of the stirrer is 300-2800 rpm / min, and the temperature of the hot silicone oil is 40-280°C.
7. The preparation method according to claim 1, characterized in that: The curing temperature in step S3 is 40-280° C. and the curing time is 0.5-48 hours.
8. The preparation method according to claim 1, characterized in that: The calcination temperature in step S5 is 200-1700° C., and the calcination time is 0.5-24 hours.