A catalyst for direct CO2 hydrogenation to ethanol and its preparation method and application
The defective ZnZrOx confined Cu-Fe bimetallic cluster catalyst was prepared by complexation-wet chemistry method, and the Cu-Fe5C2 interface structure was controlled to solve the problems of insufficient activity and selectivity of the existing catalysts and achieve efficient CO2 conversion and ethanol selection. properties, reduces preparation costs, and is suitable for industrial applications.
Patent Information
- Application Number
- CN202310444307.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-04-23
AI Technical Summary
Existing catalysts for CO2 hydrogenation to ethanol are deficient in having both excellent catalytic activity and ethanol selectivity, and the use of precious metals and cumbersome preparation methods are costly, which is not conducive to industrial application.
The defective ZnZrOx confined Cu-Fe bimetallic cluster catalyst was prepared using a complex-wet chemical method. The Cu-Fe5C2 interface structure was controlled through the defect site confinement strategy, which reduced the activation energy of the CO insertion reaction, inhibited side reactions, and improved the catalytic activity and ethanol. Selectivity.
It significantly improves the CO2 conversion rate and ethanol selectivity, reduces the production of by-product methanol, improves the stability of the catalyst, simplifies the preparation process, and is suitable for industrial applications.
Smart Images

Figure CN116474780B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to a catalyst for direct CO2 hydrogenation to ethanol, and a preparation method and application thereof. Background Art
[0002] With the rapid development of the national economy, ethanol, as an important chemical raw material and fuel, has seen a growing market demand, resulting in a situation of supply exceeding demand. In the past, ethanol was mainly produced by fermentation of crops in industry, which created a contradiction of "competing for food with the people". With the increasing prominence of global energy and environmental issues, the resource utilization of CO2 has received extensive attention from researchers in various countries. Among them, the production of ethanol by coupling CO2 with green hydrogen technology is an effective way to utilize it, which is of great strategic significance to ensuring my country's energy and food security.
[0003] Among the reaction pathways of heat, electricity, and light catalysis for CO2 hydrogenation to ethanol, heat catalysis has significant advantages such as high conversion efficiency and large-scale application. There are three main types of heat catalysts developed for CO2 hydrogenation to ethanol: (1) Precious metal catalysts. Invention patent CN113058596B discloses a CeO2-loaded Pd dimer catalyst and its use in CO2 hydrogenation to ethanol reaction. The precursor salt is mixed with the pretreated CeO2 carrier and ultrasonically dispersed, and the catalyst is obtained by washing, separation, drying, and roasting. At H2 / CO2=3:1, 240°C, 3000mL·g cat. -1 ·h -1 and 3.0MPa reaction conditions, the ethanol selectivity is 98.4%, but the CO2 conversion rate is only 4.8%. (2) Single atom catalyst. Invention patent CN115254100A discloses a supported Rh / CeTiO x Single atom catalysts and their use in CO2 hydrogenation to ethanol reaction. The active metal precursor and the metal oxide doped carrier are dispersed in an organic solvent, and the catalyst is obtained by stirring, drying and calcining. Under the reaction conditions of H2 / CO2=3:1, 250℃ and 3.0MPa, the ethanol selectivity is 99.1%, but the CO2 conversion rate is only 7.9%, and the catalyst is easily deactivated. (3) Transition metal compound catalysts, which mainly include Co-based, Cu-based, and Cu-Fe-based catalysts. The K / MoCoS catalyst prepared by the coprecipitation method has a high selectivity to ethanol at H2 / CO2=3:1, 340℃, 0.43h -1 The CO2 conversion rate was only 28.0% and the ethanol selectivity was only 5.2% under the reaction conditions of 10.4 MPa and 10.4 MPa (Catalysis Communications, 2011, Vol. 14, pp. 111-113). -1and 5.0MPa reaction conditions, the CO2 conversion rate was 17.8%, the ethanol selectivity was 5.7%, and the CH4 selectivity was 31.3% (Journal of Catalysis, 2020, Vol. 382, pp. 86-89). Invention patent CN109569712A discloses Cu@Na-Beta catalyst and its use in CO2 hydrogenation to ethanol reaction. The molecular sieve is treated with alkali solution to construct a mesoporous structure, and then the Cu salt is loaded on the molecular sieve for calcination, and then an aluminum source, a silicon source and a template are added for hydrothermal treatment, and then the catalyst is obtained by calcination and reduction. Under the reaction conditions of H2 / CO2=3:1, 300℃ and 1.3MPa, the selectivity of ethanol in organic products is about 99%, but the CO2 conversion rate is only 6.3%. The Cs-CuFeZn catalyst prepared by coprecipitation method is at H2 / CO2=3:1, 330℃, 4500mL·g cat. -1 ·h -1 and 3.0MPa reaction conditions, the CO2 conversion rate was 36.6%, but the ethanol selectivity was 24.6% (ACS Catalysis, 2020, Vol. 10, pp. 5250-5260). Although these reports focus on constructing new carriers and regulating active sites to improve ethanol selectivity or CO2 conversion rate. However, there are problems such as the inability to achieve both excellent catalytic activity and ethanol selectivity, and poor catalyst stability. In addition, the use of precious metals and the cumbersome preparation methods are costly and not conducive to industrial applications. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and to prepare defective ZnZrO by complexation-wet chemical method. x A confined Cu-Fe bimetallic cluster catalyst provides a catalyst for direct CO2 hydrogenation to ethanol and its preparation method and application.
[0005] The present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a catalyst for direct CO2 hydrogenation to ethanol, characterized in that it comprises the following steps:
[0007] S1. Preparation of defective ZnZrO x Carrier;
[0008] S2, the defective ZnZrO x The carrier is added into a solvent containing a complexing agent, and ultrasonically dispersed to form a suspension;
[0009] S3, adding a copper source and an iron source into deionized water in a certain proportion, and stirring to form a solution M;
[0010] S4, gradually adding the solution M dropwise into the suspension under stirring conditions, adjusting the pH by means of a pH-adjusting solution, and drying and calcining after stirring to obtain the catalyst.
[0011] The main reaction process of CO2 hydrogenation to ethanol on Cu-Fe-based catalysts includes: CO2 is adsorbed on Cu and activated to CO*, part of the generated CO* is activated to CH3* on Fe5C2, and then the generated CO* and CH3* undergo insertion reaction at the Cu-Fe5C2 interface, and finally hydrogenated to produce ethanol. The CO insertion reaction is the rate-determining step of the process. The side reaction process is mainly the CC coupling reaction on Fe5C2 to produce hydrocarbons, while a small amount of CO2 on Cu generates methanol via HCOO* intermediates. The activation energy of the CO insertion reaction is closely related to the Cu-Fe5C2 interface structure. However, the currently developed Cu-Fe-based catalyst preparation methods (such as impregnation, coprecipitation and hydrothermal methods) can obtain thermodynamically favorable structures, but cannot effectively regulate the Cu-Fe5C2 interface structure.
[0012] The interaction between Cu and Fe5C2 to form an interface can reduce the activation energy of CO insertion reaction, and it is also conducive to the rapid transfer of CO* generated on Cu to Fe5C2 and activated to CH3* for insertion reaction; the strong metal-support interaction can inhibit the carbonization of Fe species, and the iron carbide formed after more Fe species are carbonized can promote the formation of byproduct hydrocarbons, which is not conducive to the production of ethanol; at the same time, the small size (<7nm) of Fe5C2 is not conducive to CC coupling reaction, but can activate CO* to CH3*; hydroxyl (-OH) can stabilize formate species and protonate methanol, inhibiting the formation of methanol. The following approaches can be taken to improve the catalytic performance: (1) by constructing a Cu-Fe5C2 interface to reduce the activation energy of CO insertion reaction and strengthen the main reaction; (2) by using the strong metal-support interaction and the small size of Fe5C2 to increase the activation energy of CC coupling reaction and inhibit the side reaction; (3) by stabilizing the formation of formate species and the protonation of methanol through -OH, thereby inhibiting the formation of byproduct methanol; therefore, constructing a Cu-Fe5C2 interface with the above properties is crucial to improving catalytic activity and ethanol selectivity.
[0013] Regulating the interface structure through defect confinement strategy is a new strategy for regulating the interface structure. The defect-confined Cu-Fe bimetallic cluster catalyst has strong metal-support interaction and small size effect. At the same time, the -OH at the defect can promote the formation of intermediate species during the reaction, which can significantly improve the catalytic activity and target product selectivity in the catalytic reaction; the bimetallic clusters interact with oxygen vacancies and confine them to the carrier defects, which inhibits the formation of thermodynamically favorable structures during the activation process and promotes the formation of bimetallic interfaces.
[0014] The present invention prepares defective ZnZrO xThe carrier uses the defect site confinement strategy to promote the formation of the Cu-Fe5C2 interface. The small-sized Fe5C2 formed by the confinement effect is not conducive to the chain growth reaction, but can inhibit the formation of hydrocarbons and activate CO* to CH3*; the Cu-Fe5C2 interface has a low activation energy for the CO insertion reaction, which effectively promotes the CO insertion reaction and inhibits the chain growth reaction.
[0015] The high coverage of C1 intermediates adsorbed on the Cu surface is the key to trigger the interaction between adjacent intermediates for further CC coupling. The highly dispersed Fe5C2 nanoclusters are confined to the surface of Cu nanoparticles, forming abundant Cu-Fe5C2 interfaces. The synergistic interaction between Fe5C2 clusters and Cu nanoparticles can well promote the activation of CO2 and break the linear proportional relationship of adsorption / desorption of intermediates.
[0016] At the same time, defective ZnZrO x The hydroxyl groups on the catalyst can stabilize the formation of formate species and protonate methanol, inhibiting the production of by-product methanol. It exhibits excellent catalytic activity and ethanol selectivity in the direct CO2 hydrogenation to ethanol reaction and also has high stability.
[0017] Furthermore, step S1 is specifically as follows: dissolving the zinc source and the zirconium source in deionized water to form a solution M1, dissolving ammonium carbonate in deionized water to form a solution M2, adding the solution M1 and the solution M2 dropwise into 50-300 mL of deionized water, keeping warm at 50-90° C., aging for 5-24 hours, centrifuging, washing, and drying, and then calcining in stages in an atmosphere furnace.
[0018] Furthermore, the molar ratio of the total amount of the zinc source and the zirconium source to ammonium carbonate is 1:1-10.
[0019] Furthermore, the molar ratio of the zinc source to the zirconium source is 1:0.5-5, the zinc source is selected from one of zinc nitrate, zinc sulfate and zinc chloride; the zirconium source is selected from one of zirconium nitrate, zirconyl nitrate and zirconium acetate.
[0020] Furthermore, in step S1, the staged calcination is first calcined in an air atmosphere at 250-550°C for 4-12 hours, and then switched to a H2 / N2 atmosphere for treatment at 350-600°C for 3-10 hours, wherein the H2 content is 5-99%.
[0021] ZnZrO x Heat treatment in a reducing atmosphere causes oxygen in the crystal lattice to be separated, resulting in oxygen deficiency and the formation of oxygen vacancies.
[0022] Furthermore, in step S1, the washing is performed by using one or more of deionized water, ethanol, and methanol; and the drying is performed at 50 to 120° C. for 4 to 24 hours.
[0023] Furthermore, in step S2, the complexing agent is one or more of ethylenediaminetetraacetic acid, citric acid, diethanolamine, diethylenetriaminepentacarboxylic acid, and sodium tripolyphosphate; and the solvent is one or more of deionized water, ethanol, methanol, and toluene.
[0024] Furthermore, the molar ratio of the total amount of the copper source and the iron source to the complexing agent is 1:10-30; and the molar ratio of the copper source to the iron source is 1:0.3-5.
[0025] Furthermore, the copper source is selected from one of copper nitrate, copper sulfate, copper acetate and copper chloride; the iron source is one of iron nitrate, iron sulfate, iron chloride and iron acetate.
[0026] Furthermore, in step S4, the pH-adjusting solution is one of sodium hydroxide, hydrochloric acid, and ammonia water, and the pH is adjusted to 5-10; the drying is performed by evaporation drying at 80-120° C. on a rotary evaporator; and the calcination is performed at 350-700° C. for 4-15 hours.
[0027] The present invention also provides a catalyst for direct CO2 hydrogenation to ethanol, wherein the catalyst is a defect-confined bimetallic cluster catalyst having a Cu-Fe5C2 interface structure and is prepared by the above-mentioned preparation method.
[0028] The present invention also uses the catalyst prepared above for direct CO2 hydrogenation to ethanol. The catalyst is used for direct CO2 hydrogenation to ethanol. The catalyst reacts in a fixed bed, CO2 / H2=1:1-5, the reaction temperature is 250-400°C, the reaction pressure is 1.5-8.0MPa, and the space velocity is W / F=10-50g·mol -1 ·h -1 Ethanol was prepared under these conditions.
[0029] The present invention has the following beneficial effects:
[0030] Preparation defects of the present invention ZnZrO x The confined Cu-Fe bimetallic cluster catalyst was used for the first time in the direct CO2 hydrogenation to ethanol reaction. The defect confinement effect can promote the formation of the Cu-Fe5C2 interface. The strong interaction between the metal and the support can inhibit the carbonization of Fe species. At the same time, the size of the generated Fe5C2 is less than 7nm, which is not conducive to the chain growth reaction and inhibits the formation of hydrocarbons. The hydroxyl groups at the defect sites can stabilize the formation of formate species and the protonation of methanol, thereby inhibiting the formation of methanol, which significantly improves the CO2 conversion rate and ethanol selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 The conventional supported bimetallic catalyst and the Cu-Fe5C2 / ZnZrO x Schematic diagram of the structure of cluster catalyst;
[0033] Figure 2 The Cu-Fe5C2 / ZnZrO prepared in Example 1 of the present invention x HR-TEM image of the cluster catalyst. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention provides a method for preparing a catalyst for direct CO2 hydrogenation to ethanol, characterized in that it comprises the following steps:
[0036] S1. Preparation of defective ZnZrO x Carrier;
[0037] S2, the defective ZnZrO x The carrier is added into a solvent containing a complexing agent, and ultrasonically dispersed to form a suspension;
[0038] S3, adding a copper source and an iron source into deionized water in a certain proportion, and stirring to form a solution M;
[0039] S4, gradually adding the solution M dropwise into the suspension under stirring conditions, adjusting the pH by means of a pH-adjusting solution, and drying and calcining after stirring to obtain the catalyst.
[0040] Specifically, step S1 is: dissolving a zinc source and a zirconium source in deionized water to form a solution M1, dissolving ammonium carbonate in deionized water to form a solution M2, adding solution M1 and solution M2 dropwise into 50-300 mL of deionized water, keeping warm at 50-90° C., aging for 5-24 hours, centrifuging, washing, and drying, and then calcining in stages in an atmosphere furnace.
[0041] As a preferred solution, the molar ratio of the total amount of the zinc source and the zirconium source to the ammonium carbonate is 1:1 to 10;
[0042] As a further preferred scheme, the molar ratio of the zinc source to the zirconium source is 1:0.5-5, the zinc source is selected from one of zinc nitrate, zinc sulfate and zinc chloride; the zirconium source is selected from one of zirconium nitrate, zirconyl nitrate and zirconium acetate.
[0043] Among them, in step S1, the washing adopts one or more of deionized water, ethanol, and methanol; the drying is dried at 50-120°C for 4-24 hours; the staged calcination is first calcined at 250-550°C in an air atmosphere for 4-12 hours, and then switched to a H2 / N2 atmosphere and treated at 350-600°C for 3-10 hours, wherein the H2 content is 5-99%.
[0044] Specifically, in step S2, the complexing agent is one or more of ethylenediaminetetraacetic acid, citric acid, diethanolamine, diethylenetriaminepentacarboxylic acid, and sodium tripolyphosphate; and the solvent is one or more of deionized water, ethanol, methanol, and toluene.
[0045] Specifically, the molar ratio of the total amount of the copper source and the iron source to the complexing agent is 1:10-30; the molar ratio of the copper source to the iron source is 1:0.3-5, the copper source is selected from one of copper nitrate, copper sulfate, copper acetate, and copper chloride; the iron source is one of iron nitrate, iron sulfate, iron chloride, and iron acetate.
[0046] Specifically, in step S4, the pH-adjusting solution is one of sodium hydroxide, hydrochloric acid, and ammonia water, and the pH is adjusted to 5-10; the drying is performed by evaporation drying at 80-120° C. on a rotary evaporator; and the calcination is performed at 350-700° C. for 4-15 hours.
[0047] The catalyst for direct CO2 hydrogenation to ethanol prepared by the present invention is a defect-confined bimetallic cluster catalyst with a Cu-Fe5C2 interface structure, which can be applied to direct CO2 hydrogenation to ethanol. The specific process is: the catalyst reacts in a fixed bed, CO2 / H2=1:1-5, the reaction temperature is 250-400°C, the reaction pressure is 1.5-8.0MPa, and the space velocity is W / F=10-50g·mol -1 ·h -1 Ethanol was prepared under these conditions.
[0048] The present invention adopts complexation-wet chemical method to prepare defective ZnZrO x Confined Cu-Fe bimetallic cluster catalyst, its structure is as follows Figure 1 (right figure) as shown, compared with Figure 1 The structure of the traditional supported bimetallic catalyst shown in the left figure isx The Cu-Fe5C2 interface is formed by the defect confinement strategy. The small Fe5C2 formed by the confinement effect is not conducive to the chain growth reaction and can inhibit the formation of hydrocarbons, but can activate CO* to CH3*. The Cu-Fe5C2 interface has a low activation energy for CO insertion reaction, which effectively promotes CO insertion reaction and inhibits chain growth reaction. x The hydroxyl groups on the catalyst can stabilize the formation of formate species and protonate methanol, inhibiting the production of by-product methanol. It exhibits excellent catalytic activity and ethanol selectivity in the direct CO2 hydrogenation to ethanol reaction and also has high stability.
[0049] The present invention will be further described below by the following specific embodiments:
[0050] Example 1
[0051] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0052] (1) In a molar ratio of n(zinc+zirconium):n(ammonium carbonate)=1:5, zinc nitrate and zirconium oxynitrate were dissolved in deionized water to form solution M1, and ammonium carbonate was dissolved in deionized water to form solution M2. Then, solution M1 and solution M2 were uniformly added dropwise to a beaker containing 200 mL of deionized water under stirring, kept at 60°C, aged for 14 hours, centrifuged, washed with deionized water, dried at 120°C for 10 hours, and then calcined at 400°C in an air atmosphere for 5 hours, and then switched to a 10% H2 / N2 atmosphere and treated at 500°C for 6 hours to obtain defective ZnZrO x Carrier;
[0053] (2) At a molar ratio of n(Cu+Fe):n(complexing agent) = 1:30, the defective ZnZrO x The carrier is added into deionized water dissolved with ethylenediaminetetraacetic acid, and ultrasonically dispersed to form a suspension;
[0054] (3) adding copper nitrate and iron nitrate into deionized water at a ratio of n(Cu):n(Fe)=1:1 and stirring for 1 h to form solution M;
[0055] (4) The solution M obtained in step (3) was added dropwise to the suspension formed in step (2) under stirring, and sodium hydroxide was added dropwise to adjust the pH to 7.5, stirred for 3 h, and then evaporated to dryness on a rotary evaporator at 100 ° C, and calcined at 400 ° C for 5 h to obtain a defect-confined cluster catalyst, recorded as Cu-Fe5C2 / ZnZrO x .
[0056] The Cu-Fe5C2 / ZnZrO prepared in Example 1 was observed by high resolution transmission electron microscopy (HR-TEM). xThe cluster catalyst was characterized and the results are shown in Figure 2 As shown. Figure 2 It can be seen that there is an obvious interface between Cu and Fe5C2, indicating that the defect confinement strategy can promote the formation of Cu-Fe5C2 interface.
[0057] Example 2
[0058] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0059] (1) Same as Example 1;
[0060] (2) At a molar ratio of n(Cu+Fe):n(complexing agent) = 1:20, the defective ZnZrO x The carrier is added into an ethanol solution containing ethylenediaminetetraacetic acid, and ultrasonically dispersed to form a suspension;
[0061] (3) adding copper chloride and ferric chloride into deionized water at a ratio of n(Cu):n(Fe)=1:1 and stirring for 1 h to form solution M;
[0062] (4) The solution M obtained in step (3) is added dropwise to the suspension formed in step (2) under stirring, and aqueous ammonia is added to adjust the pH to 7.5. The mixture is stirred for 4 h, and then evaporated to dryness at 120 ° C on a rotary evaporator, and calcined at 550 ° C for 6 h to obtain a defect-confined cluster catalyst.
[0063] Example 3
[0064] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0065] (1) In a molar ratio of n(zinc+zirconium):n(ammonium carbonate)=1:8, zinc nitrate and zirconium oxynitrate were dissolved in deionized water to form solution M1, and ammonium carbonate was dissolved in deionized water to form solution M2. Then, solution M1 and solution M2 were uniformly added dropwise to a beaker containing 300 mL of deionized water under stirring, kept at 80°C, aged for 24 hours, centrifuged, washed with deionized water, dried at 100°C for 12 hours, and then calcined at 500°C in an air atmosphere for 6 hours, and then switched to a 99% H2 atmosphere and treated at 500°C for 8 hours to obtain defective ZnZrO x Carrier;
[0066] (2) Same as Example 1;
[0067] (3) Same as Example 1;
[0068] (4) The solution M obtained in step (3) is added dropwise to the suspension formed in step (2) under stirring, and hydrochloric acid is added to adjust the pH to 6. The mixture is stirred for 4 hours, and then evaporated to dryness on a rotary evaporator at 100° C. and calcined at 600° C. for 8 hours to obtain a defect-confined cluster catalyst.
[0069] Example 4
[0070] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0071] (1) Same as Example 1;
[0072] (2) At a molar ratio of n(Cu+Fe):n(complexing agent) = 1:10, the defective ZnZrO x The carrier is added into a deionized water solution containing citric acid and ultrasonically dispersed to form a suspension;
[0073] (3) adding copper nitrate and iron nitrate into deionized water at a ratio of n(Cu):n(Fe)=1:3 and stirring for 1 h to form solution M;
[0074] (4) The solution M obtained in step (3) is added dropwise to the suspension formed in step (2) under stirring, and hydrochloric acid is added to adjust the pH to 6.5, and stirred for 6 hours, and then evaporated to dryness on a rotary evaporator at 100° C., and calcined at 500° C. for 6 hours to obtain a defect-confined cluster catalyst.
[0075] Example 5
[0076] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0077] (1) Same as Example 1;
[0078] (2) At a molar ratio of n(Cu+Fe):n(complexing agent) = 1:10, the defective ZnZrO x The carrier is added into a methanol solution containing diethylenetriaminepentacarboxylic acid, and ultrasonically dispersed to form a suspension;
[0079] (3) adding copper acetate and ferric acetate into deionized water at a ratio of n(Cu):n(Fe)=1:2 and stirring for 2 h to form solution M;
[0080] (4) Same as Example 4.
[0081] Example 6
[0082] The catalyst for direct CO2 hydrogenation to ethanol was prepared by the following steps:
[0083] (1) Same as Example 4;
[0084] (2) At a molar ratio of n(Cu+Fe):n(complexing agent) = 1:20, the defective ZnZrO x The carrier is added into a deionized water solution containing diethylenetriaminepentacarboxylic acid, and ultrasonically dispersed to form a suspension;
[0085] (3) Same as Example 1;
[0086] (4) The solution M obtained in step (3) is added dropwise to the suspension formed in step (2) under stirring, sodium hydroxide is added to adjust the pH to 8, stirred for 4 hours, then evaporated to dryness at 80° C. on a rotary evaporator, and calcined at 600° C. for 5 hours to obtain a defect-confined cluster catalyst.
[0087] Comparative Example 1
[0088] In step (3) of Example 1, no iron source is added, and the rest of the preparation method is the same as steps (1), (2) and (4) in Example 1.
[0089] Comparative Example 2
[0090] In step (3) of Example 1, no copper source is added, and the rest of the preparation method is the same as steps (1), (2) and (4) in Example 1.
[0091] Comparative Example 3
[0092] In a molar ratio of n(Cu+Fe):n(sodium carbonate)=1:5, copper nitrate and ferric nitrate are dissolved in deionized water to form solution M1, and sodium carbonate is dissolved in deionized water to form solution M2, and then solution M1 and solution M2 are uniformly added dropwise into a beaker filled with 300 mL of deionized water under stirring, kept warm at 60°C, pH=8, aged for 24 hours, centrifuged, washed with deionized water, dried at 100°C for 12 hours, and then calcined at 400°C in an air atmosphere for 6 hours to obtain a catalyst.
[0093] Test example
[0094] The catalysts prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were pelletized into 20 to 40 meshes, and 0.5 g was taken and loaded into a micro high-pressure fixed bed reactor to evaluate its catalytic performance in catalyzing CO2 hydrogenation to ethanol. The test conditions refer to the aforementioned "Specific application method of the catalyst in the reaction". 0.5 g of the catalyst was loaded into a micro fixed bed reactor, wherein the catalyst activation conditions were: gas 10% CO / N2, pressure 0.1 MPa, flow rate 40 mL min -1 , heating rate 2°·min -1 , 350℃ pretreatment for 8h, and then the catalytic performance was evaluated at CO2 / H2=1:3, reaction temperature 320℃, reaction pressure 5.0MPa, space velocity W / F=45g·mol -1 ·h -1Direct CO2 hydrogenation to ethanol reaction was carried out under the conditions of , and the results are shown in Tables 1 and 2.
[0095] Table 1 Catalytic performance of the catalysts prepared in Examples 1 to 6
[0096]
[0097] Table 2 Catalytic performance of catalysts prepared in Comparative Examples 1 to 3
[0098]
[0099] From the comparison between Table 1 and Table 2, it can be seen that the Cu-Fe5C2 interface cannot be formed in Comparative Examples 1 and 2, and the catalyst of Comparative Example 3 has no carrier and exists in the form of a composite metal oxide, and no Cu-Fe5C2 interface is formed, indicating that not adopting the defect confinement strategy is not conducive to the formation of the Cu-Fe5C2 interface, and a large amount of hydrocarbons are generated in the CO2 hydrogenation reaction, and the ethanol selectivity is low. Therefore, the defect ZnZrO x The confinement effect of the carrier and the formation of the Cu-Fe5C2 interface have a considerable influence on the activity and ethanol selectivity of the catalyst.
[0100] It can be seen from Table 1 that compared with the developed catalytic system, the CO2 conversion rate and ethanol selectivity of the present invention are greatly improved, and the methanol selectivity is low. The preparation method of the catalyst of the present invention is simple, easy to promote and apply in industry, and has potential economic value. Compared with other structural catalysts, the Cu-Fe5C2 interface structure and size effect can promote the CO insertion reaction to inhibit chain growth ability, and significantly improve the catalytic activity and ethanol selectivity.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for direct CO 2 A method for preparing a catalyst for hydrogenating ethanol, It is characterized in that The following steps are involved: S1. Preparation of defective ZnZrO x Carrier: Dissolve the zinc source and the zirconium source in deionized water to form a solution M1, dissolve ammonium carbonate in deionized water to form a solution M2, add the solution M1 and the solution M2 dropwise into 50-300 mL of deionized water, keep warm at 50-90° C., age for 5-24 hours, centrifuge, wash, dry, and then roast in an atmosphere furnace in stages, wherein the molar ratio of the total amount of the zinc source and the zirconium source to the ammonium carbonate is 1:1-10; In step S1, the staged calcination is firstly calcined at 250-550°C in air atmosphere for 4-12h, and then switched to H 2 / N 2 The mixture is treated at 350-600℃ for 3-10h in H 2 The content is 5-99%; S2, the defective ZnZrO x The carrier is added into a solvent containing a complexing agent, and ultrasonically dispersed to form a suspension; S3, adding a copper source and an iron source into deionized water in a certain proportion, and stirring to form a solution M; S4. Gradually drop the solution M into the suspension under stirring conditions, adjust the pH by means of a pH-adjusting solution, dry and calcine after stirring to obtain the catalyst, wherein the molar ratio of the total amount of the copper source and the iron source to the complexing agent is 1:10-30; and the molar ratio of the copper source to the iron source is 1:0.3-5.
2. The method for direct CO 2 A method for preparing a catalyst for hydrogenating ethanol, Features: The molar ratio of the zinc source to the zirconium source is 1:0.5-5, the zinc source is selected from one of zinc nitrate, zinc sulfate and zinc chloride; the zirconium source is selected from one of zirconium nitrate, zirconyl nitrate and zirconium acetate.
3. The method for direct CO 2 A method for preparing a catalyst for hydrogenating ethanol, Features: In step S2, the complexing agent is one or more of ethylenediaminetetraacetic acid, citric acid, diethanolamine, diethylenetriaminepentacarboxylic acid, and sodium tripolyphosphate; and the solvent is one or more of deionized water, ethanol, methanol, and toluene.
4. The method for direct CO 2 A method for preparing a catalyst for hydrogenating ethanol, Features: In step S4, the pH-adjusting solution is one of sodium hydroxide, hydrochloric acid and ammonia water, and the pH is adjusted to 5-10; the drying is performed by evaporation drying at 80-120° C. on a rotary evaporator; and the calcination is performed at 350-700° C. for 4-15 hours.
5. A method for direct CO 2 Catalyst for hydrogenation to ethanol, Features: The catalyst is a defect-confined bimetallic cluster catalyst with Cu-Fe 5 C 2 The interface structure is prepared by the method described in any one of claims 1 to 4.
6. A method for direct CO 2 Application of catalysts for hydrogenation to ethanol, Features: The catalyst reacts in a fixed bed, CO 2 / H 2 =1:1~5, reaction temperature is 250~400℃, reaction pressure is 1.5~8.0MPa, space velocity is W / F=10~50g·mol -1 ·h -1 Ethanol is prepared under the following conditions; the catalyst is the catalyst according to claim 5.